Dissolving gold with HCl/Cl2

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

goldandsilver123

Well-known member
Joined
Aug 11, 2015
Messages
206
The first experiment using HCl/Cl2 to dissolve gold.

The pressure was around 7 cm of water column at around 40ºC.

https://www.youtube.com/watch?v=dprkRtNuiOc

WhatsApp Image 2018-09-17 at 20.35.52.jpeg

WhatsApp Image 2018-09-17 at 20.35.54.jpeg

20 g of pure gold, time to dissolve ~1:30 H

* the first hose is PTFE the other ones are silicone and were thrown away after.
 
FrugalRefiner said:
I like the color. How much HCl did you use?

Dave

100 mL of 6 molar HCl + ~20 mL 37% for the addition funnel


Direct Video:
[youtube]http://www.youtube.com/watch?v=dprkRtNuiOc[/youtube]
 
It appears that I am in love with chlorine.

Wonder if the gas house will let me order a small cylinder.




Sent from my iPhone using Tapatalk
 