I can't seem to depopulate these circuit boards

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

JBo

Member
Joined
Mar 17, 2018
Messages
23
Hi everyone. I spent about 48 hours trying to depopulate 500g of these clean cut circuit boards by doing a standard AP solution with 31.45% muriatic acid and 2% HCl in a 3:1 ratio respectively. I poured muriatic acid onto the circuit boards until the acid covered the top boards by about 1 cm, and then added 1/3 of the volume HCL I used of Muratic acid. But I can't even get a quarter of the boards clean after trying to run an aquarium pump through. Could someone give me a suggestion?
 

Attachments

  • IMG_3212.JPG
    IMG_3212.JPG
    2.3 MB · Views: 227
  • IMG_3213.JPG
    IMG_3213.JPG
    2.2 MB · Views: 227
  • IMG_3214.JPG
    IMG_3214.JPG
    1.7 MB · Views: 227
JBo said:
Hi everyone. I spent about 48 hours trying to depopulate 500g of these clean cut circuit boards by doing a standard AP solution with 31.45% muriatic acid and 2% HCl in a 3:1 ratio respectively.
Did you make a mistake in typing this? AP stands for acid/peroxide. Muriatic acid and HCl are the same thing.

You also say you are trying to "depopulate" the boards. When we talk about depopulating boards, it refers to removing components like integrated circuits, surface mount components, etc. from the boards. I'm assuming you are actually trying to remove the gold foils from the boards.

Assuming you really used muriatic acid and hydrogen peroxide, you used too much peroxide. You only need a tiny amount, like a capful, to get the process started. The AP process is slow. Depending on other factors it can take days, weeks, or even months to dissolve the copper layer between the circuit board and the gold plating.

Dave
 
As above, use an air bubbler and add an aquarium heater to the bucket, AP is very temperature dependent.

Also, those are likely ENIG gold over Copper, do you know how to process the gallons of toxic Copper waste you will create for a tiny amount of Gold ?
 
This plating is so thin you will likely not see any foils but it rather disintegrates to tiny specs and powder like. If I would have to guess I would say less than a gram worth of gold there.
Give it about a week or two of soaking and check again. It also helps to stir them once or twice a day to make sure they are not stuck together and acid gets to all of the surfaces.
 
Dave,

Whoops. Yeah I miss typed. I meant Muratic acid (HCl) and 2% hydrogen peroxide.
Thanks for the advice! I'll add less hydrogen peroxide. I'm a newbie if you can't tell :)

Also, do you think it's even worth processing these if they are ENIG? How much gold can I possible get fro them if I have 8.7 pounds of it?
 