Post by cuchugold » March 15th, 2019, 9:43 am

Hi guys. My daughter has shown some artful/acute interest in jewellery, and I helped her with the basic colors of alloys yellow, red/pink, and green. I'm interested in any comments from people that have actually worked with the blue and purple types shown in the bottom of this table:
https://www.thoughtco.com/composition-o ... oys-608016

Cheers and thanks in advance.
"Life gets better when we can make life easier for others - do something nice for someone today". KA.
"The difference between a dream & reality is, a good plan!...and execution thereof." PhilD & HAuCl4
"It is always impossible, till it is done".
"Is the juice worth the squeeze?".

User avatar
philddreamer
Active Member
Posts: 2189
Joined: February 12th, 2010, 12:02 am
Country of Origin: USA
Location: Lynnwood, WA.

Re: Colored alloys of gold.

Post by philddreamer » March 16th, 2019, 2:08 pm

Maybe some good info here...
viewtopic.php?f=33&t=22551&p=236299&hil ... oy#p236299

Take care!

Phil
If you are going to dream... DREAM BIG!!!
You may say that I'm a dreamer... but I'm not the only one!
"Paper money eventually returns to its intrinsic value --- zero." Voltaire (1694-1778)
The difference between a dream & reality is, a good plan!
WARNING: No "cartridge type" respirator will filter out nitric fumes, NONE!!!

Keepper1
Member
Posts: 2
Joined: April 1st, 2019, 5:04 am
Country of Origin: japan

Re: Colored alloys of gold.

Post by Keepper1 » April 1st, 2019, 5:10 am

Hello. I am a new member. Nice to meet everyone.

User avatar
cuchugold
Active Member
Posts: 242
Joined: October 25th, 2017, 6:37 am
Country of Origin: Bananistan

Re: Colored alloys of gold.

Post by cuchugold » April 2nd, 2019, 6:16 am

philddreamer wrote:
March 16th, 2019, 2:08 pm
Maybe some good info here...
viewtopic.php?f=33&t=22551&p=236299&hil ... oy#p236299

Take care!

Phil
Thanks Phild. I've done a dozen experimental attempts at the blue (iron+gold), and 5 at the purple (aluminium + gold), and have not gotten a workable jewellery alloy yet. I've put this aside for now. The other alloys are fairly easily obtained.
"Life gets better when we can make life easier for others - do something nice for someone today". KA.
"The difference between a dream & reality is, a good plan!...and execution thereof." PhilD & HAuCl4
"It is always impossible, till it is done".
"Is the juice worth the squeeze?".

goldandsilver123
Active Member
Posts: 114
Joined: August 11th, 2015, 3:22 pm
Country of Origin: Brazil

Re: Colored alloys of gold.

Post by goldandsilver123 » April 3rd, 2019, 9:30 am

I've made the "blue" gold alloy. 75% gold 25% iron.
You cannot roll it, I tried and it shattered.

I melted in a eletric furnace under melted borax, must keep O2 away.

The alloy is grey, the blue color comes from an oxide layer from heat treatment. It was like 30s in 500°C oven.
Label clearly. Measure twice. Eat elsewhere.

Lou
Active Member
Posts: 4497
Joined: November 4th, 2007, 5:28 pm
Country of Origin: USA
Location: Rhodia Drive

Re: Colored alloys of gold.

Post by Lou » April 3rd, 2019, 11:47 am

A more easily attained blue with indium instead.

Most of these are in fact intermetallics, hence their brittle nature.
Like chemistry? Try http://sciencemadness.org/talk

All that glitters is not gold. Occasionally it's rhodium :)

grainsofgold
Active Member
Posts: 152
Joined: May 28th, 2007, 11:08 pm
Country of Origin: USA
Location: USA

Re: Colored alloys of gold.

Post by grainsofgold » April 3rd, 2019, 7:26 pm

Google PM west Refining n Ca call and ask for Daniel -

He has cast purple gold and can give you detailed info -

nickvc
Active Member
Posts: 4304
Joined: September 14th, 2009, 10:53 am
Country of Origin: England
Location: birmingham

Re: Colored alloys of gold.

Post by nickvc » April 4th, 2019, 4:53 am

All I can add to your search is that the little I know of those colours of gold is that they are very brittle and working them will be near impossible but casting may well produce a usable piece, the alloys made are very similar in my mind to gold contaminated with 5% or more pgms which fracture very easily.
I knew someone who spent a lot of time trying to make purple gold for inlays into rings and who failed miserably, I wonder whether it could be machined carefully if a rod or bar could be produced, scrap rates would be horrendous so that the items would be very expensive.

User avatar
cuchugold
Active Member
Posts: 242
Joined: October 25th, 2017, 6:37 am
Country of Origin: Bananistan

Re: Colored alloys of gold.

Post by cuchugold » April 7th, 2019, 6:49 am

Thanks all for the responses.
"Life gets better when we can make life easier for others - do something nice for someone today". KA.
"The difference between a dream & reality is, a good plan!...and execution thereof." PhilD & HAuCl4
"It is always impossible, till it is done".
"Is the juice worth the squeeze?".

Post Reply