Retorting/gold/silver amalgamation

Post by Sheilareid » March 17th, 2019, 3:07 am

I retorted impregnated mercury for the first time,I now have a clump of gold and silver amalgamation.how do I desperate them?

User avatar
anachronism
Active Member
Posts: 2258
Joined: May 31st, 2016, 2:51 am
Country of Origin: England

Re: Retorting/gold/silver amalgamation

Post by anachronism » March 17th, 2019, 5:40 am

Sheilareid wrote:
March 17th, 2019, 3:07 am
I retorted impregnated mercury for the first time,I now have a clump of gold and silver amalgamation.how do I desperate them?
If you retorted it you should have split the amlagum into mercury and a mix of gold/silver.

How come you still have mercury mixed? Can you show us the retort you used?

I'm sure plenty of people will be along to tell you how you shouldn't be doing this but let's fix your problem too.
If you keep on doing what you've always done then you'll just keep on getting what you've always got.

"If you can bear to hear the truth you’ve spoken twisted by knaves to make a trap for fools, or watch the things you gave your life to broken, and stoop and build ‘em up with wornout tools" -- Rudyard Kipling

"The best diplomat that I know is a fully-loaded phaser bank." -- Lt. Cdr. Montgomery Scott

kernels
Active Member
Posts: 556
Joined: April 14th, 2016, 7:12 am
Country of Origin: New Zealand
Location: Auckland, New Zealand

Re: Retorting/gold/silver amalgamation

Post by kernels » March 17th, 2019, 10:30 pm

So, retorting basically boils off the Mercury (which you hopefully condensed and collected), so it sounds like you are saying you now have a clumpy mixture of Gold and Silver.

The simplest solution is to add some more silver (melt) to ensure that Gold only makes up 25% max of the mixture, then use Nitric acid to separate Gold from Silver.

Bacially, you want to look at the inquartation Process.

Sheilareid
Member
Posts: 3
Joined: February 15th, 2019, 11:18 am
Country of Origin: United States

Re: Retorting/gold/silver amalgamation

Post by Sheilareid » March 27th, 2019, 5:04 am

Thank you for the advice.I am new to this site,and haven't figured out posting pictures yet.The retort I have is about 40 years old,but it does fine as far as recovering the mercury.but I ended up with a hard button of silver and gold when I was finished.I just inherited 24 gold claims from my dad.(1-6 ounces
per ton).He worked it for close to 40 years.i have alot to learn.

Sheilareid
Member
Posts: 3
Joined: February 15th, 2019, 11:18 am
Country of Origin: United States

Re: Retorting/gold/silver amalgamation

Post by Sheilareid » March 27th, 2019, 5:07 am

I incorrectly worded my original problem.The amalgam was of mercury,gold,and I assume silver.After I retorted the amalgam,I was left with a clump of...gold and ..silver? I am confused as to how I desperate the gold.

User avatar
FrugalRefiner
Active Member
Posts: 3806
Joined: January 14th, 2012, 5:06 pm
Country of Origin: USA
Location: Ohio, USA

Re: Retorting/gold/silver amalgamation

Post by FrugalRefiner » March 27th, 2019, 7:34 am

Sheilareid wrote:
March 27th, 2019, 5:04 am
Thank you for the advice.I am new to this site,and haven't figured out posting pictures yet.
See Attaching Images or Files, Working with Attachments.

Dave
Printer friendly copy of C. M. Hoke's Refining Precious Metal Wastes.
Screen readable copy of C. M. Hoke's Refining Precious Metal Wastes.

Platdigger
Active Member
Posts: 1598
Joined: July 26th, 2007, 1:48 am
Location: Washington

Re: Retorting/gold/silver amalgamation

Post by Platdigger » March 27th, 2019, 10:47 am

Just curious here and not meaning to muddy the waters but,

how sure can one be that All, and I mean All the mercury is gone after retorting?

You know, if you go to melt this clump and there is any mercury left, there it goes into the atmosphere and surrounding area.

User avatar
FrugalRefiner
Active Member
Posts: 3806
Joined: January 14th, 2012, 5:06 pm
Country of Origin: USA
Location: Ohio, USA

Re: Retorting/gold/silver amalgamation

Post by FrugalRefiner » March 27th, 2019, 11:46 am

It is never all gone. There will always be at least a trace of mercury left in the button.

Dave