lazersteve
Well-known member
I've decided to post a new tutorial on recovering silver metal from silver chloride. I posted the segment on how to separate silver from gold with dilute nitric acid which yielded silver chloride. You can view that post here:
http://goldrefiningforum.com/phpBB3/viewtopic.php?p=887&highlight=#887
I'll be posting two parts to this topic one for the electolytic method and the other for the purely chemical method.
The quick overview is as folows:
1. Electrolytic Precipitation of Silver from Silver Chloride
Cathode: Graphite
Anode: Platinum Wire
Electrolyte: Ammonium Hydroxide and Silver Chloride
Product Retrival: Vaccuum Filtration of Powder Residue
Clean Up: Distilled water wash.
Smelting: Use borax flux
Product Purity: 99%+
2. Hydroxide Precipitation of Silver from Silver Chloride
UPDATE This tutorial is now available at :
http://goldrefiningforum.com/phpBB3/viewtopic.php?p=1208#1208
Chemicals: Dry Sodium Hydroxide
Corn Syrup
Distilled Water
Silver Chloride
Product Retrival: Filtration of Powder Residue
Clean Up: Distilled water wash.
Smelting: Use borax flux
Product Purity: 98%+
I'll begin these videos when I finish up with the last filtering video.
Please post your suggestions and comments.
Steve
http://goldrefiningforum.com/phpBB3/viewtopic.php?p=887&highlight=#887
I'll be posting two parts to this topic one for the electolytic method and the other for the purely chemical method.
The quick overview is as folows:
1. Electrolytic Precipitation of Silver from Silver Chloride
Cathode: Graphite
Anode: Platinum Wire
Electrolyte: Ammonium Hydroxide and Silver Chloride
Product Retrival: Vaccuum Filtration of Powder Residue
Clean Up: Distilled water wash.
Smelting: Use borax flux
Product Purity: 99%+
2. Hydroxide Precipitation of Silver from Silver Chloride
UPDATE This tutorial is now available at :
http://goldrefiningforum.com/phpBB3/viewtopic.php?p=1208#1208
Chemicals: Dry Sodium Hydroxide
Corn Syrup
Distilled Water
Silver Chloride
Product Retrival: Filtration of Powder Residue
Clean Up: Distilled water wash.
Smelting: Use borax flux
Product Purity: 98%+
I'll begin these videos when I finish up with the last filtering video.