Post subject: Refining Using Butyl DiglymePosted: April 29th, 2007, 4:49 pm
Site Admin
Joined: February 24th, 2007, 7:10 pm
Posts: 2916
Location: Sherbrooke, Qc Butyl Diglyme is a good variation of the standard Aqua Regia method. You can achieve a gold purity of 99,99+ with BDG. Also, BDG is reusable.
This tutorial will show you how to refine gold using it.
Material:
-Butyl Diglyme (go there if you plan to buy some: http://goldrefining.110mb.com/phpBB2/viewtopic.php?t=99)
-Separatory Funnel (Very very useful. Take a 2L funnel if possible.)
-Hot plate
-Gold Chloride (dissolved gold)
-Oxalic Acid or other precipitant.
-Standard PPE
-HCl
-Water
-Scale
-Magnetic Stirrer (optional)
Here is the tutorial link:
http://goldrefining.110mb.com/Tutorials/BDG%20refining.htm
Questions or Comments:
http://goldrefining.110mb.com/phpBB2/viewtopic.php?p=5455#5455
[img::]http://i14.tinypic.com/4xzt7kg.jpg[/img]
Very pure gold achieved with BDG.
_________________
Hallmarks are lies.
Last edited by Noxx on June 27th, 2007, 7:50 pm, edited 1 time in total.
Noxx: Would it be possible to restore the links in your post? I would like to see them if possible. I read as much on refining as I can find and this has me curious.
Thanks, Mark
Site Admin
Joined: February 24th, 2007, 7:10 pm
Posts: 2916
Location: Sherbrooke, Qc Butyl Diglyme is a good variation of the standard Aqua Regia method. You can achieve a gold purity of 99,99+ with BDG. Also, BDG is reusable.
This tutorial will show you how to refine gold using it.
Material:
-Butyl Diglyme (go there if you plan to buy some: http://goldrefining.110mb.com/phpBB2/viewtopic.php?t=99)
-Separatory Funnel (Very very useful. Take a 2L funnel if possible.)
-Hot plate
-Gold Chloride (dissolved gold)
-Oxalic Acid or other precipitant.
-Standard PPE
-HCl
-Water
-Scale
-Magnetic Stirrer (optional)
Here is the tutorial link:
http://goldrefining.110mb.com/Tutorials/BDG%20refining.htm
Questions or Comments:
http://goldrefining.110mb.com/phpBB2/viewtopic.php?p=5455#5455
[img::]http://i14.tinypic.com/4xzt7kg.jpg[/img]
Very pure gold achieved with BDG.
_________________
Hallmarks are lies.
Last edited by Noxx on June 27th, 2007, 7:50 pm, edited 1 time in total.
Noxx: Would it be possible to restore the links in your post? I would like to see them if possible. I read as much on refining as I can find and this has me curious.
Thanks, Mark