Well-known member
Joined
Aug 14, 2018
Messages
60
Location
Calgary AB
Hello everyone.
I'd like to start a new thread called AP Gold Pin Process question.
I've only started reining on a small scale for a few months. I have done a few small batches of low grade (25 grams), medium grade (35 grams) and my last batch, high grade gold pins (60 grams) All mixed non magnetic.

The first few batches were a bit tedious while separating the foils from the pins.
The base metals would dissolve about 50% and 85% of the pins would be stripped.
I would pour off as much as I could through a filter which emptied into a used AP jug, then I would transfer the filter to a water rinsing container and spray the gold pin bearing container through the filter.

But as you guys probably already know it's tough to separate gold foils from small dissolving pins. And adding water to these pins only created white crystals which dissolved with a bit of hcl. Since I have a few 1 liter jugs of used AP I now use them to add more liquid to the high grade pin container to decant. I now swish it around and decant into the foil beaker. And do that a few times until the majority of the foils are out.
Then added more Hcl to dissolve the remaining foils. A few days later when 99% of the base metals from the pins dissolved I decanted and picked out the 3 or 4 small pins that didn't dissolve.

With the last batch of high grade gold pins (60 grams, non magnetic mixed pins) I just let them sit for a few extra days until 99% of the pins had dissolved. (4 days in total)
I didn't filter any of the solution, after reading more on here I thought it wise to only use the filter once after dissolving the gold.
I ended up decanting the pin bath several times into my 1000 ml beaker, using the used AP solution and then sprayed out the container with water into the same beaker.
After waiting a day I still see lots of gold floating through out the solution. Could you guys suggest a way for the gold to settle?
And if my procedures were incorrect and inefficient please do shine some light.
I plan on dissolving the foils in this beaker and dropping the gold with Smb. Saving the powder until I find the means to melt efficiently.

Ps. I bought this beaker at a brewery supply store for $17. It doesn't say Pyrex, or anything to do with heat. Is anyone familiar with this beaker, and it's it safe to boil with?

Thanks!
Peter
 

Attachments

  • 20180822_082324.jpg
    20180822_082324.jpg
    5 MB · Views: 459
  • 20180822_082336.jpg
    20180822_082336.jpg
    3.7 MB · Views: 459
Beaker
https://www.veegee.com/products/glassware/beakers/20229-50-vee-gee-50-ml-beaker-847.html

Erlenmeyer flask
https://www.veegee.com/20231-1000-vee-gee-1000-ml-erlenmeyer-flask.html
 
Sheesh, that was of course a few clicks for me to find myself. Thank you for finding that! Looks to be just as good if not better (cheaper) than Pyrex. I'll see what I can do about getting a few different sizes of this type.
 
PARKER113 said:
Could you guys suggest a way for the gold to settle?

Hit the floaters with a mist of water from a spray bottle. If they are still too oily to sink you can dab a tiny amount of dish soap onto the end of a stir stick and just touch it to the surface of the solution. It will lower the surface tension and you should see the foils drop pretty quickly.

A quick incineration prior to processing will burn the ois off the pins and take care of the problem beforehand.

PARKER113 said:
safe to boil with?

Sure, but keep in mind that with the narrowing neck of the flask that a vigorous or runaway reaction will boil over A LOT faster than it would with a straight sided beaker.
 
PARKER113 said:
Sheesh, that was of course a few clicks for me to find myself. Thank you for finding that! Looks to be just as good if not better (cheaper) than Pyrex. I'll see what I can do about getting a few different sizes of this type.

I was showing you those links because what you were calling a beaker was not a beaker. it's an erlenmeyer flask. A beaker is much easier to pour out of (decant) and also much, much easier to remove the solids. The beaker is more general purpose and the flask is good for specific things - it will concentrate the heat better.
 
I never fill my Erlenmeyer more than 1/4 full. Beakers are also easier to clean. Unclebenben's drop of soap and a spray bottle works for me.
 
Thanks for the reply guys.
Hehe I did not know the difference between a beaker and Erlenmeyer flask. It makes a lot of sense to use a beaker for the majority of the e scrap process. I need to modify my glass stir sticks so they don't damage the glass. Rubber tubing from aquarium pump I'm thinking.

As far as the gold settling. Thank you for your suggestions. But the fine gold seems the same weight as the solution almost. As in a small amount of foils are suspended all the way up. It's now been about two days. Is possible the solution has too many metals?

Also I have no means as of yet to incinerate.. Unless I can make something with some basic ingenuity. What I did with the last batch of pins wash wash them in 70% alcohol. Hoping that would remove the majority of grime.

Thanks!

Peter
 
PARKER113 said:
small amount of foils are suspended all the way up.

I see. Floating in, not on. Then yes, your solution is getting saturated. Good chance there is some tin gelling it up a bit. Hard to completely avoid when dissolving whole pins. If a drop of water creates a white cloud of
copper(I)chloride, it's saturated with copper and time to decant and replace the acid. Filter to catch the floating foils. Save them to add with the majority of foils when you get done dissolving all the pins.

The alcohol wash will help. By incinerate I mean just put the pins in an old skillet and play a light flame from a propane torch over them to burn off organics. (Never use the skillet for food again!)

Good luck, Peter. Stay safe.
 
UncleBenBen said:
By incinerate I mean just put the pins in an old skillet and play a light flame from a propane torch over them to burn off organics. (Never use the skillet for food again!)
As Ben said. I like a stainless steel skillet/fry pan. You can pick one up at the Goodwill/St. Vincent DePaul/second hand store for a few dollars. In a perfect world, you can put it on an old propane burner like the ones used as a side burner on a lot of propane grills. Get it well heated, then play a torch over the top. You don't want it so hot that things melt, just a dull red heat to burn off all the organics.

Dave
 
Hi Dave,
I have a large stainless steel shallow skillet that would work wonderfully. I don't have a barbeque but if I layer the pins thin enough on the skillet the flame should incinerate the majority of the organics. Then maybe shake it up and go over it again.

Thanks for your input!

Peter
 
That will work.

I'm a charcoal man myself. Never used a propane grill to cook food. But since I've been refining, I've acquired a couple. People throw them away or give them away all the time, often for minor problems. The side burners on the ones I've gotten have always worked. It's a frugal way to get a propane burner. 8)

Dave
 
When I was doing foils I would use a charmin plug to get the floaties. I know a drop of dish soap has been recommended a lot through the forum. But if you dont ridden the foils later on of excess soap. You can make some foam or potential boil over with sparkles.

If you dont have a grill or even a cheap torch. I got a small toaster oven as a burnout oven, for $5 at a goodwill. Wal-Mart, Kmart, Goodwill, and other places with baking stuff had mini stoneware breadloaf pans. Only $3....They work really well and slicker than snot. Good for incinerating powders too.

Andrew
 
Thanks for the recommendation guys! I do have a max pro torch so that should work. Also I have a decent electric burner.
New person question probably.. I finally got the TIN II (100 grams)stannous chloride from the chemical supply store $140.00 with the hazardous handing charge.. I'll attach a pic. But how do I make the test solution? I added about a gram of it to some hcl and dissolved it. Tested it on some gold solutions and it didn't react. After further reading.. Do I need to add tin pieces and distilled water aswell?

Thanks,

Peter
 

Attachments

  • 20180825_134805.jpg
    20180825_134805.jpg
    4.3 MB · Views: 302
Yes, you should add some distilled water. Lou suggested 1 gram SnCl2 dihydrate, 5 ml HCl, and 20 ml distilled water. Add some metallic tin to keep the solution in good condition.

That's a crazy price for stannous chloride.

Dave
 
FrugalRefiner said:
Yes, you should add some distilled water. Lou suggested 1 gram SnCl2 dihydrate, 5 ml HCl, and 20 ml distilled water. Add some metallic tin to keep the solution in good condition.

That's a crazy price for stannous chloride.

Dave

Agreed the money would have been better spent buying some decent glassware, he could have got some tin solder or fishing sinkers for a few dollars and made his own :shock:
 
https://www.ebay.com/itm/Stannous-Chloride-Anhydrous-99-8-1-4-lb/312222149574?hash=item48b1e3ebc6:g:VRcAAOxyoahSWxR~

I think this is the guy I bought from the last time. About $20 including shipping for 113g
 
The price is probably due to "Certified ACS suitable for mercury determination".

Interesting note, it also says "Will absorb oxygen from the air, and convert to the insoluble oxychloride. Keep tightly closed."
This is what happens in solution too when stannous goes bad.

Göran
 
Thanks for the insight guys.
I did invest in a few more good glassware items a few days ago so I'm pretty happy about that! Also bought a corningware piece that had held up to the element quite well.
I tested it with water first and wasn't able to bring it to a boil with the set up I have. Not that I'm looking to boil, but I don't know if I'm getting the high temperature I need to wash the gold. Bubbles appear at the bottom and come up well. The solution is hot. (I think it's due to the sand I'm using) gold mining sand still.
I ended up dissolving the foils I got from my 60 grams of high grade pins a few days ago with bleach and let it sit for a day.
Then used my element to heat up the solution to better drop the gold. The first time I tried nothing was dropping (It's 10 degrees Celsius) outside. So I heated it up and it worked well. Maybe a gram or so of gold.

Well I'll never buy the stannous chloride for that much again! Way to expensive. Should last a few years though.
 

Attachments

  • 20180828_171204.jpg
    20180828_171204.jpg
    4.7 MB · Views: 213
  • 20180828_171200.jpg
    20180828_171200.jpg
    4.7 MB · Views: 213
  • 20180819_133434.jpg
    20180819_133434.jpg
    3.8 MB · Views: 213
g_axelsson said:
The price is probably due to "Certified ACS suitable for mercury determination".

Interesting note, it also says "Will absorb oxygen from the air, and convert to the insoluble oxychloride. Keep tightly closed."
This is what happens in solution too when stannous goes bad.

Göran

Would putting in an oxygen absorber be useful?
 