• Please join our new sister site dedicated to discussion of gold, silver, platinum, copper and palladium bar, coin, jewelry collecting/investing/storing/selling/buying. It would be greatly appreciated if you joined and help add a few new topics for new people to engage in.

    Bullion.Forum

Non-Chemical 50 pounds of ICs, the results, and how I did it

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

JaMora

Member
Joined
Jul 12, 2021
Messages
11
Location
Somewhere
Okay, so here are the results of 1.5 years of saving up 50 pounds of mixed integrated chips (including BGAs).

Before you read the result below, it is important to note that most of the chips (90%) were from 1990s to early 2000s automotive electronics. Meaning these were not super modern electronics and most likely were higher component quality.

Roughly 50 pounds of mixed chips yielded 83 grams of gold.

Below are the exact amounts (quantity and weight) of different styles of ICs. The 'Gold Return' column is estimated. Keep in mind, I did not weigh each individual yield after burning, sieving on a shaker table, and thereafter collecting ash and using a blue bowl. Instead, I completed the entire process of 50 pounds and weighed the results at the end. What I’m saying is, I initially had an estimated yield for each style of chip based on internet resources, and after getting the result of 83 grams, I fixed my estimates to equal the true 83-gram result. The total result in the table is slightly over the actual result as there were most likely losses in the blue bowl portion of the process.

Pins per sideThicknessStyle (Size & Thickness)Est. Gold Per KgTotal Weight (Kilograms)Gold Return (Grams)
1SThickThrough-hole Chips1.52.53.75
2SThickLegacy 2-sided Chips2.51.53.75
2SThickMedium to Large sized thick 2-sided chips3412
4SThickMedium to Large sized Legacy Flatpack/PLCC CPUs3.56.723.45
2S & 4SThinSmall Mixed ICs & Transistors428
4SThickMedium-size, Thick Rectangular & Square Chips4.52.511.25
2S & 4SThinSmall to Medium sized, Thin mixed Chips616
4SThinLarge sized, Thin Flatpack CPUs8.50.54.25
BGABGASmall BGA & RAM Chips (AP to remove tin)10.50.55.25
BGABGAGold Corner BGA Chips (tops only)14.50.57.25
21.784.95


I decided to go the Burning method as this was safer than using chemicals. Burning off the volatiles to “reduce” the epoxy to carbon. I wanted not to disturb the bonding wires as much as possible along the way of liberating them from the wafers/pins. I know ball mills and coffee grinders would work, but the sieve and shaker system seemed best for minimal losses.

Before getting into how I processed the chips, some notes on what I learned along the way.

  • If using the shaker table/sieving process, there is no need to use AP to remove pins/legs from chips as sieving will do the work. I found that NO pins were able to pass through the 120 mesh (125um) sieve.
  • Most pins will be trapped in the 18 and 35 mesh sieves.
  • I did use AP on small BGA chips to get rid of tin.
  • Shaker table and sieving seemed to liberate even the smallest amounts of gold as large quantities of gold dust was found in the blue bowl along with bonding wires. This dust was not something I've seen people get in all the videos of other methods.
  • A small hobby kiln for glass is key to completely pyrolyzing chips that don't fall apart after shaking in glass jar.
  • If you use a hobby kiln to pyrolyze chip pieces that do not break apart during shaking/sieving, make sure to not heat for too long or you will melt copper pins and make a mess and possibly fuse bonding wires to metallics. The kiln I used had a timer, I always put it to 8 minutes.
PROCESS:

1. First, incineration of ICs (combustion, presence of oxygen) in a controlled combustion using a propane torch - the kind for burning weeds. Burn chips in stainless steel, high-sided cake pan, in a simple fire brick box. Continue to heat while gently mixing until all visible black carbon turns white, and smoking stops. Burn a little at a time to ensure smoke does not escape the burning vessel. I always burned 1 kg of chips at a time, starting with a few handfuls in the pan and throwing in small handfuls as I burned. I used a military issued gas mask during this process and would do it with nothing of lesser quality. Usually takes about 15 minutes and very little smoke if you take your time and have a hot propane torch.

2. Put the burned chips in a large glass container and manually shake like hell (about 3 mins of shaking).

3. Sieve using 8 in diameter sieves. Below are the only sizes needed for this process. Place IC ash into top test sieve in stack and put on small shaker table (bought from Amazon - Vibro Pro Kinetic - works well for this process but pricey). The stack of sieves is held still on the shaker table using a large wood working clamp. Its kind of loud but not too bad.
-18 mesh - 1mm
-35 mesh - 500 um
-120 mesh- 125 um
-Catch Pan

4. Use a hobby glass kiln to further pyrolyze pieces of chips that do not break into ash. Begin picking out metallic parts (pins and heatsinks) out of top sieve. After that, pull out the larger pieces of ICs and place into small stainless-steel dish and place the dish into the kiln (small hobby glass kiln bought from Amazon). Pyrolyze pieces of chips that do not pass through the sieve and shake in a glass container once again before putting ash back into the sieve set on the shaker table. Repeat this process until everything passes through each sieve and the bottom catch pan of the sieve set has nothing but ash and bonding wires. You will have picked out most of the larger metallic pieces along the way. At certain points you can just empty the sieve of metallic pieces when all ash passes through. Know that, not all pieces of chips will make it through 120 mesh sieve, for example, after going through 50 pounds of chips, I was left with about 2 cups of ‘ash’ that would simply not break apart small enough to pass through the 120 mesh sieve regardless of pyrolyzing and shaking. I will probably need to actually grind that up in a coffee grinder (which I haven't done yet)

5. Wash off the fine (ash) by method of choice to provide a “concentrate” before using a final common method to wash/separate ash from gold bonding wires (panning, blue bowl, sluice box/table, etc.). I used Successful Engineer’s method in one of his last videos on YouTube regarding gold recovery as his method was the best I'd come across. I used a 7-gallon drywall bucket to hold the water mixed with ash with a small cement mixer on my cordless drill and a little Jetdry. A spigot placed 1 inch up from the bottom of the bucket, draining via small hose to a small handheld sluice, leading to another smaller bucket with excess water spilling over second buckets edge. I processed roughly one gallon of ash each time I used this method, I probably could have done more at a time - but wanted to play it safe. Most importantly, were the time intervals after mixing the ash in water to let gold settle to the bottom - 30 mins, 20 mins, 10 mins, 5 mins. Watch his videos for the details. I pretty much did the same as him, but used a bigger drywall bucket and different style mini sluice between the buckets. I found very little gold losses in second bucket using his method. Seriously great idea on Successful Engineer's behalf. I can’t help but to facepalm when I see people doing the other bucket method, pouring from one bucket to the other. Yikes.

6. I used a Blue Bowl setup exactly like Successful Engineer’s setup. In his videos, he had to deal with some metallic pins as he did not use the 120-mesh sieve which would have caught all metallic pins. Since I did, I only had to deal with ash and gold in the blue bowl. Some tips: You must concentrate the IC ash, or you will be at the blue bowl forever haha. Do not remove the gold bonding wires/dust from blue bowl as you go along – I found that keeping them in the bowl helped keep other bonding wires from washing out of the bowl, especially the longer bonding wires from gold corner BGAs. Take your time. If your in a rush, you have the wrong hobby :)

Hope this helps the community. Bye!
 
Last edited:
Use a magnifying glass and look through the pins..... you could have bonding wires that will still be attacked/bound up on the pins. Probably not a huge amount but why throw out gold. When I have IC legs I put them in a separate bucket. Each time I process my PM stock pot, I put that solution in with pins before I move the solution to Cu recovery bucket loaded with iron. Over time those pins will slooowly dissolve leaving behind the bonding wires. No need to create anymore waste solutions to deal with, plus you can recover the Cu from the pins...... if that's your thing.

How many Lbs/Kilo's of pins did you end up with?


PS.... When I say slooowly, that is a big understatement.
 
I checked the pins with a small handheld microscope (out of curiosity) during every 1 kilo batch I processed. I did confirm there was bonding wires still attached after initially shaking incinerated chips in the glass jar.

Using the same handheld microscope, I constantly checked pins after they would shake on the vibration table for a few 10 minute iterations of shaking/sieving. I was never able to find a bonding wire still attached to a pins after the first two rounds of the vibration/shaker table. I think this is due to the amount of shaking the content goes through. Especially in vibrating against the metal sieve mesh screen. Plus I put a few small ball bearings in the sieves to encourage bouncing (more vibration). Long story short, bonding wires attached to pins seems not to be an issue in using this method. Trust me, I tried to find them still attached, but nope!

I had the same curiosity for the silicon dies - they never had bonding wires - even the gold weld spots on the dies were missing after the shaking/sieving process - I would bet all of the gold dust I had in the blue bowl in addition to the bonding wires were from these 'weld' points on the pins and dies where the gold bonding wires were attached. I would also bet, I would have lost all of the gold dust if I had not implemented the correct washing method learned from Successful Engineer's YouTube channel.

However, there was quiet a few heatsinks and pins that were gold plated. I did keep all metals pulled out of sieves in a big 1.5 liter glass jar. I'll weigh them now... the glass jar filled to the brim weighs 9 pounds (including the jar). Also, I did previously remove all of the chunky copper heat sinks from the through-hole 1-sided ICs and threw those to the copper bucket - that would have made the overall weight much more.

My best friend owns an automotive junk yard - As a hobby, I get all the automotive computers/electronics and take the gold stuff and give everything back to him so he can get it processed in the future (automotive electronics utilize a lot of PGMs) - I'll be putting these pins in his gaylord box with all of the boards I give back to him for his own benefit :) No PMs in the trash haha.
 
Last edited:
Awesome.... I assume your going to share pic's of the gold button/bar at some point?

You already addressed it, but my next reply was about the silicon die's. Very little gold on the die's, but they are so easy to process...why not get it.
 
Gives me hope that it’s worth filling this 5 gallon bucket before I process them.

Thanks. Great write up.
 
Okay, so here are the results of 1.5 years of saving up 50 pounds of mixed integrated chips (including BGAs).

Before you read the result below, it is important to note that most of the chips (90%) were from 1990s to early 2000s automotive electronics. Meaning these were not super modern electronics and most likely were higher component quality.

Roughly 50 pounds of mixed chips yielded 83 grams of gold.

Below are the exact amounts (quantity and weight) of different styles of ICs. The 'Gold Return' column is estimated. Keep in mind, I did not weigh each individual yield after burning, sieving on a shaker table, and thereafter collecting ash and using a blue bowl. Instead, I completed the entire process of 50 pounds and weighed the results at the end. What I’m saying is, I initially had an estimated yield for each style of chip based on internet resources, and after getting the result of 83 grams, I fixed my estimates to equal the true 83-gram result. The total result in the table is slightly over the actual result as there were most likely losses in the blue bowl portion of the process.

Pins per sideThicknessStyle (Size & Thickness)Est. Gold Per KgTotal Weight (Kilograms)Gold Return (Grams)
1SThickThrough-hole Chips1.52.53.75
2SThickLegacy 2-sided Chips2.51.53.75
2SThickMedium to Large sized thick 2-sided chips3412
4SThickMedium to Large sized Legacy Flatpack/PLCC CPUs3.56.723.45
2S & 4SThinSmall Mixed ICs & Transistors428
4SThickMedium-size, Thick Rectangular & Square Chips4.52.511.25
2S & 4SThinSmall to Medium sized, Thin mixed Chips616
4SThinLarge sized, Thin Flatpack CPUs8.50.54.25
BGABGASmall BGA & RAM Chips (AP to remove tin)10.50.55.25
BGABGAGold Corner BGA Chips (tops only)14.50.57.25
21.784.95


I decided to go the Burning method as this was safer than using chemicals. Burning off the volatiles to “reduce” the epoxy to carbon. I wanted not to disturb the bonding wires as much as possible along the way of liberating them from the wafers/pins. I know ball mills and coffee grinders would work, but the sieve and shaker system seemed best for minimal losses.

Before getting into how I processed the chips, some notes on what I learned along the way.

  • If using the shaker table/sieving process, there is no need to use AP to remove pins/legs from chips as sieving will do the work. I found that NO pins were able to pass through the 120 mesh (125um) sieve.
  • Most pins will be trapped in the 18 and 35 mesh sieves.
  • I did use AP on small BGA chips to get rid of tin.
  • Shaker table and sieving seemed to liberate even the smallest amounts of gold as large quantities of gold dust was found in the blue bowl along with bonding wires. This dust was not something I've seen people get in all the videos of other methods.
  • A small hobby kiln for glass is key to completely pyrolyzing chips that don't fall apart after shaking in glass jar.
  • If you use a hobby kiln to pyrolyze chip pieces that do not break apart during shaking/sieving, make sure to not heat for too long or you will melt copper pins and make a mess and possibly fuse bonding wires to metallics. The kiln I used had a timer, I always put it to 8 minutes.
PROCESS:

1. First, incineration of ICs (combustion, presence of oxygen) in a controlled combustion using a propane torch - the kind for burning weeds. Burn chips in stainless steel, high-sided cake pan, in a simple fire brick box. Continue to heat while gently mixing until all visible black carbon turns white, and smoking stops. Burn a little at a time to ensure smoke does not escape the burning vessel. I always burned 1 kg of chips at a time, starting with a few handfuls in the pan and throwing in small handfuls as I burned. I used a military issued gas mask during this process and would do it with nothing of lesser quality. Usually takes about 15 minutes and very little smoke if you take your time and have a hot propane torch.

2. Put the burned chips in a large glass container and manually shake like hell (about 3 mins of shaking).

3. Sieve using 8 in diameter sieves. Below are the only sizes needed for this process. Place IC ash into top test sieve in stack and put on small shaker table (bought from Amazon - Vibro Pro Kinetic - works well for this process but pricey). The stack of sieves is held still on the shaker table using a large wood working clamp. Its kind of loud but not too bad.
-18 mesh - 1mm
-35 mesh - 500 um
-120 mesh- 125 um
-Catch Pan

4. Use a hobby glass kiln to further pyrolyze pieces of chips that do not break into ash. Begin picking out metallic parts (pins and heatsinks) out of top sieve. After that, pull out the larger pieces of ICs and place into small stainless-steel dish and place the dish into the kiln (small hobby glass kiln bought from Amazon). Pyrolyze pieces of chips that do not pass through the sieve and shake in a glass container once again before putting ash back into the sieve set on the shaker table. Repeat this process until everything passes through each sieve and the bottom catch pan of the sieve set has nothing but ash and bonding wires. You will have picked out most of the larger metallic pieces along the way. At certain points you can just empty the sieve of metallic pieces when all ash passes through. Know that, not all pieces of chips will make it through 120 mesh sieve, for example, after going through 50 pounds of chips, I was left with about 2 cups of ‘ash’ that would simply not break apart small enough to pass through the 120 mesh sieve regardless of pyrolyzing and shaking. I will probably need to actually grind that up in a coffee grinder (which I haven't done yet)

5. Wash off the fine (ash) by method of choice to provide a “concentrate” before using a final common method to wash/separate ash from gold bonding wires (panning, blue bowl, sluice box/table, etc.). I used Successful Engineer’s method in one of his last videos on YouTube regarding gold recovery as his method was the best I'd come across. I used a 7-gallon drywall bucket to hold the water mixed with ash with a small cement mixer on my cordless drill and a little Jetdry. A spigot placed 1 inch up from the bottom of the bucket, draining via small hose to a small handheld sluice, leading to another smaller bucket with excess water spilling over second buckets edge. I processed roughly one gallon of ash each time I used this method, I probably could have done more at a time - but wanted to play it safe. Most importantly, were the time intervals after mixing the ash in water to let gold settle to the bottom - 30 mins, 20 mins, 10 mins, 5 mins. Watch his videos for the details. I pretty much did the same as him, but used a bigger drywall bucket and different style mini sluice between the buckets. I found very little gold losses in second bucket using his method. Seriously great idea on Successful Engineer's behalf. I can’t help but to facepalm when I see people doing the other bucket method, pouring from one bucket to the other. Yikes.

6. I used a Blue Bowl setup exactly like Successful Engineer’s setup. In his videos, he had to deal with some metallic pins as he did not use the 120-mesh sieve which would have caught all metallic pins. Since I did, I only had to deal with ash and gold in the blue bowl. Some tips: You must concentrate the IC ash, or you will be at the blue bowl forever haha. Do not remove the gold bonding wires/dust from blue bowl as you go along – I found that keeping them in the bowl helped keep other bonding wires from washing out of the bowl, especially the longer bonding wires from gold corner BGAs. Take your time. If your in a rush, you have the wrong hobby :)

Hope this helps the community. Bye!
Thanks for sharing your methodology. It may help many members.
 
Okay, so here are the results of 1.5 years of saving up 50 pounds of mixed integrated chips (including BGAs).

Before you read the result below, it is important to note that most of the chips (90%) were from 1990s to early 2000s automotive electronics. Meaning these were not super modern electronics and most likely were higher component quality.

Roughly 50 pounds of mixed chips yielded 83 grams of gold.

Below are the exact amounts (quantity and weight) of different styles of ICs. The 'Gold Return' column is estimated. Keep in mind, I did not weigh each individual yield after burning, sieving on a shaker table, and thereafter collecting ash and using a blue bowl. Instead, I completed the entire process of 50 pounds and weighed the results at the end. What I’m saying is, I initially had an estimated yield for each style of chip based on internet resources, and after getting the result of 83 grams, I fixed my estimates to equal the true 83-gram result. The total result in the table is slightly over the actual result as there were most likely losses in the blue bowl portion of the process.

Pins per sideThicknessStyle (Size & Thickness)Est. Gold Per KgTotal Weight (Kilograms)Gold Return (Grams)
1SThickThrough-hole Chips1.52.53.75
2SThickLegacy 2-sided Chips2.51.53.75
2SThickMedium to Large sized thick 2-sided chips3412
4SThickMedium to Large sized Legacy Flatpack/PLCC CPUs3.56.723.45
2S & 4SThinSmall Mixed ICs & Transistors428
4SThickMedium-size, Thick Rectangular & Square Chips4.52.511.25
2S & 4SThinSmall to Medium sized, Thin mixed Chips616
4SThinLarge sized, Thin Flatpack CPUs8.50.54.25
BGABGASmall BGA & RAM Chips (AP to remove tin)10.50.55.25
BGABGAGold Corner BGA Chips (tops only)14.50.57.25
21.784.95


I decided to go the Burning method as this was safer than using chemicals. Burning off the volatiles to “reduce” the epoxy to carbon. I wanted not to disturb the bonding wires as much as possible along the way of liberating them from the wafers/pins. I know ball mills and coffee grinders would work, but the sieve and shaker system seemed best for minimal losses.

Before getting into how I processed the chips, some notes on what I learned along the way.

  • If using the shaker table/sieving process, there is no need to use AP to remove pins/legs from chips as sieving will do the work. I found that NO pins were able to pass through the 120 mesh (125um) sieve.
  • Most pins will be trapped in the 18 and 35 mesh sieves.
  • I did use AP on small BGA chips to get rid of tin.
  • Shaker table and sieving seemed to liberate even the smallest amounts of gold as large quantities of gold dust was found in the blue bowl along with bonding wires. This dust was not something I've seen people get in all the videos of other methods.
  • A small hobby kiln for glass is key to completely pyrolyzing chips that don't fall apart after shaking in glass jar.
  • If you use a hobby kiln to pyrolyze chip pieces that do not break apart during shaking/sieving, make sure to not heat for too long or you will melt copper pins and make a mess and possibly fuse bonding wires to metallics. The kiln I used had a timer, I always put it to 8 minutes.
PROCESS:

1. First, incineration of ICs (combustion, presence of oxygen) in a controlled combustion using a propane torch - the kind for burning weeds. Burn chips in stainless steel, high-sided cake pan, in a simple fire brick box. Continue to heat while gently mixing until all visible black carbon turns white, and smoking stops. Burn a little at a time to ensure smoke does not escape the burning vessel. I always burned 1 kg of chips at a time, starting with a few handfuls in the pan and throwing in small handfuls as I burned. I used a military issued gas mask during this process and would do it with nothing of lesser quality. Usually takes about 15 minutes and very little smoke if you take your time and have a hot propane torch.

2. Put the burned chips in a large glass container and manually shake like hell (about 3 mins of shaking).

3. Sieve using 8 in diameter sieves. Below are the only sizes needed for this process. Place IC ash into top test sieve in stack and put on small shaker table (bought from Amazon - Vibro Pro Kinetic - works well for this process but pricey). The stack of sieves is held still on the shaker table using a large wood working clamp. Its kind of loud but not too bad.
-18 mesh - 1mm
-35 mesh - 500 um
-120 mesh- 125 um
-Catch Pan

4. Use a hobby glass kiln to further pyrolyze pieces of chips that do not break into ash. Begin picking out metallic parts (pins and heatsinks) out of top sieve. After that, pull out the larger pieces of ICs and place into small stainless-steel dish and place the dish into the kiln (small hobby glass kiln bought from Amazon). Pyrolyze pieces of chips that do not pass through the sieve and shake in a glass container once again before putting ash back into the sieve set on the shaker table. Repeat this process until everything passes through each sieve and the bottom catch pan of the sieve set has nothing but ash and bonding wires. You will have picked out most of the larger metallic pieces along the way. At certain points you can just empty the sieve of metallic pieces when all ash passes through. Know that, not all pieces of chips will make it through 120 mesh sieve, for example, after going through 50 pounds of chips, I was left with about 2 cups of ‘ash’ that would simply not break apart small enough to pass through the 120 mesh sieve regardless of pyrolyzing and shaking. I will probably need to actually grind that up in a coffee grinder (which I haven't done yet)

5. Wash off the fine (ash) by method of choice to provide a “concentrate” before using a final common method to wash/separate ash from gold bonding wires (panning, blue bowl, sluice box/table, etc.). I used Successful Engineer’s method in one of his last videos on YouTube regarding gold recovery as his method was the best I'd come across. I used a 7-gallon drywall bucket to hold the water mixed with ash with a small cement mixer on my cordless drill and a little Jetdry. A spigot placed 1 inch up from the bottom of the bucket, draining via small hose to a small handheld sluice, leading to another smaller bucket with excess water spilling over second buckets edge. I processed roughly one gallon of ash each time I used this method, I probably could have done more at a time - but wanted to play it safe. Most importantly, were the time intervals after mixing the ash in water to let gold settle to the bottom - 30 mins, 20 mins, 10 mins, 5 mins. Watch his videos for the details. I pretty much did the same as him, but used a bigger drywall bucket and different style mini sluice between the buckets. I found very little gold losses in second bucket using his method. Seriously great idea on Successful Engineer's behalf. I can’t help but to facepalm when I see people doing the other bucket method, pouring from one bucket to the other. Yikes.

6. I used a Blue Bowl setup exactly like Successful Engineer’s setup. In his videos, he had to deal with some metallic pins as he did not use the 120-mesh sieve which would have caught all metallic pins. Since I did, I only had to deal with ash and gold in the blue bowl. Some tips: You must concentrate the IC ash, or you will be at the blue bowl forever haha. Do not remove the gold bonding wires/dust from blue bowl as you go along – I found that keeping them in the bowl helped keep other bonding wires from washing out of the bowl, especially the longer bonding wires from gold corner BGAs. Take your time. If your in a rush, you have the wrong hobby :)

Hope this helps the community. Bye!
Hello, I happen to stumble across your post and have been searching the net through in and throughout for automotive car components and recovery and this helps me greatly. Is the ECM and BCM (if you can recall) the only computers/modules you've gone through to get ICS or what would you say be the best modules to go for if you can recall for ICS? I have so many questions lol.
 
Hello, I happen to stumble across your post and have been searching the net through in and throughout for automotive car components and recovery and this helps me greatly. Is the ECM and BCM (if you can recall) the only computers/modules you've gone through to get ICS or what would you say be the best modules to go for if you can recall for ICS? I have so many questions lol.
Welcome to us.
 
It would be nice if you lay out your plans ahead.
Collecting and selling or processing.
What about your background.
How much studies of the subject have you done and so on.
Well in my state it's hard to get precious metals from electronics as the competition beats me to it for the most part. On the side when I'm doing car work I found precious metals exist in cars and I'm always in and out of junkyards for customers. So people overlook car components for easy recovery of valuable metals. Right now I am looking into little fuses that are common in cars and overlooked as they have silver/tin plating. Running an experiment here within a week or so to get a solid confirmation if the automotive fuses have half and half or more silver than tin. I know car relays exist with silver contacts as well and there's a YouTuber with info on that. I have not searched the forum to the exact point just yet seeing that there is a vast knowledge to sift through with the search guide lol. So I plan to add my knowledge in-between being a father and have collected quite a bit of electronic components to get an okay yield.
 
Well in my state it's hard to get precious metals from electronics as the competition beats me to it for the most part. On the side when I'm doing car work I found precious metals exist in cars and I'm always in and out of junkyards for customers. So people overlook car components for easy recovery of valuable metals. Right now I am looking into little fuses that are common in cars and overlooked as they have silver/tin plating. Running an experiment here within a week or so to get a solid confirmation if the automotive fuses have half and half or more silver than tin. I know car relays exist with silver contacts as well and there's a YouTuber with info on that. I have not searched the forum to the exact point just yet seeing that there is a vast knowledge to sift through with the search guide lol. So I plan to add my knowledge in-between being a father and have collected quite a bit of electronic components to get an okay yield.
Well there are many components containing PMs and not all are obvious.

Anyway since it seems you plan to process I recommend you to study these links.

We ask our new members to do 3 things.
1. Read C.M. Hokes book on refining jewelers scrap, it gives an easy introduction to the most important chemistry regarding refining.
It is free here on the forum: https://goldrefiningforum.com/phpBB3/viewtopic.php?f=54&t=19798
2. Then read the safety section of the forum: https://goldrefiningforum.com/forums/safety.47/
3. And then read about "Dealing with waste" in the forum: https://goldrefiningforum.com/threads/dealing-with-waste.10539/

Suggested reading:
https://goldrefiningforum.com/forums/the-library.101/
https://goldrefiningforum.com/threads/when-in-doubt-cement-it-out.30236/
https://goldrefiningforum.com/threa...le-read-this-before-you-post-about-ore.33333/


Forum rules is here.
https://goldrefiningforum.com/threads/gold-refining-forum-rules.31182/
 
Familiar with hokes refining book as it was referred from sreetips videos to download the PDF for free and read the book 😁. He is one of my favorite hobbyist refiners on YouTube for thorough start to finish of processing refining and waste management with safety and so on of years of watching him and many others across the globe.
 


Write your reply...

Latest posts

Back
Top