First Post, first silver bars!

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

Gsracer

Well-known member
Joined
Dec 21, 2020
Messages
154
Well since the pandemic like many others ive been looking for a new hobby, so silver. Ive been reading on this forum for a while and decided to finally join. This place is a great resource to learn and i have really enjoyed reading many posts and threads, and have watched numerous videos by sreetips. I'm not at refining just yet however, well... see below.

I've been collecting silver for a while mostly bullion and 90% junk coins and of course that became a Segway to sterling silver of which I have acquired to this date about 300 troy ounces of sterling, overall I've averaged about 16.00 per troy ounce of sterling, given the pandemic prices i don't think I've done too bad. Again this is just a hobby so I'm not trying to build a fortune here.

I've been recently categorizing and making sets out of what i can, being a lover of history some of the stuff i cant bring myself to destroy so when i can i resell it typically way above melt in hopes that the person buying it will use it and perhaps give some of these items another 100 years of life.

However this post is not about processiong silver as im not there yet, but i wanted to try my hand at melting some of the sterling which was too far gone to be saved.

I purchased a propane furnace, graphite crucible and some graphite molds and decided to melt about 50 troy ounces of the stuff into bars.

Now i had never done this before but i do weld and fabricate so i had some experience with molten metal.

My first attempt at bars went quite well, id really like to improve the outcome of some of the bars, maybe get the ripple pour as i have seen some of you guys do but i haven't been able to get there just yet.

Heres my process, again i had no experience doing this just what i gathered from reading here and other places.

My process is pretty much clean the silver ware with soap and water. Place into the crucible. When’s the metal is molten around 1900 degrees I shut off the furnace. Sprinkle about a table spoon of borax and remove, I usually get a few impurities out. Stir with a graphite rod and continue to heat. My pour temperature is around 2100-2200 degrees and I am pouring into the preheated molds with a map torch on top then quenching. I am seeing a melt loss off between 1.25-2.25%.

Here is some pics

The 3 small bars are between 10.2 and 10.8 troy and the big one i dont know as it maxes out my scale. I speculate its between 15-20 troy. I have some outgassing on the top of a few.

Any tips to help me improve would be appreciated.

Thank you all.
 

Attachments

  • 1.jpg
    1.jpg
    384.4 KB · Views: 345
  • 2.jpg
    2.jpg
    426.1 KB · Views: 345
  • 3.jpg
    3.jpg
    512.2 KB · Views: 345
forgot the pics of the bars
 

Attachments

  • 4.jpg
    4.jpg
    547 KB · Views: 340
  • 6.jpg
    6.jpg
    397.5 KB · Views: 339
  • 7.jpg
    7.jpg
    654.3 KB · Views: 342
  • 8.jpg
    8.jpg
    338.2 KB · Views: 342
  • 9.jpg
    9.jpg
    336.1 KB · Views: 342
Maybe I am missing something, or I just do not understand?
Are you just melting metals or did you refine the silver?

From what I understand you are taking easily recognized and stamped sterling silver and melting it into an unrecognizable block of sterling silver that is harder to sell for its value than the scrap was?
Why melt it into a bar?
Why not just sell the scrap as it was (marked or recognized for its value), or if you must melt it then why not just melt then pouring it into cold water to make beads and small chunks or a shot of the sterling, and then refine it with nitric acid and then an electrolytic cell?
 
Gsracer said:
Any tips to help me improve would be appreciated.

Thank you all.

In my opinion your bars/pours look VERY NICE considering your set up & method --- or to put it another way I would call the bars/pours a job "well done"

About the only way you will get better looking pours would be to set up to do your melts & pours in an oxygen free set up - which is something you really don't need worry about unless you are wanting to produce a 5 nine pure silver that is an oxygen free product

So outside of setting up to produce a 5 nine (99999) oxygen free product you are already producing a well done product (IMO)

Kurt
 
butcher said:
From what I understand you are taking easily recognized and stamped sterling silver and melting it into an unrecognizable block of sterling silver that is harder to sell for its value than the scrap was?

Per the underlined - As much as that advice is "often" given here on the forum --- it is only true "to a point"

The question is where/how you intend to sell your silver

IF (the big IF) you intend to take your silver to the local pawn shop &/or local coin dealer/shop (that also buys metals as scrap) then yes - they like to see the un-melted as is "marked" scrap

That is because their testing methods are limited so their testing methods are really nothing more then to confirm that the metal is in fact what it is marked as --- in other words (most) of their testing methods only give a "ball park" result of purity - so if you melt it (no longer has an identifying mark) they no longer have a true confirmation of test against the object as marked - therefore they are likely to ding you on the pay out because you could have added "a bit" of copper to the melt so they are going to want to pay out at the "low" end of their ball park test --- example; - when melted they may only want to pay out as 900 silver instead of 925 silver --- or - they may suspect that the silver was poured around a "filler metal" in the center of the bar & therefore not want to buy at all

So yes - if selling to pawn shops or coin dealers you are better off taking the scrap in "as is" with the markings stamped on the scrap because their tests are done to confirm the metal is "as marked"

On the other hand - if you intend to sell direct to a refinery then it doesn't matter because they are going to do a melt & a "true" assay on the melt anyway --- you just need to make sure everything you put in your melt is in fact true to as marking --- therefore you need to do the confirmation (acid) testing of everything you put in your melt before sending to the refinery

Why melt it into a bar?

Because (especially when dealing with silver) you can save anywhere from quite a bit to a LOT in shipping cost by melting into bars --- that's because melted bars take up MUCH less space in a box then the same weight of a bunch of "as is" sterling items --- in other words what can take 2 or 3 larger boxes of sterling "as is" items to ship - can be reduced to one "flat rate" box by melting to bars

Example; - a few years ago I had a little over 1,200 ozt sterling - about half of it was large items like serving tray's, bowls & cups with the other half mostly flatware (spoons, forks & knife "handles") & even though I had smashed all the bowls & cups down with a hammer & even folded the platers (hammered flat) it still took up 3 large boxes (about 2 1/2 to 3 cubic foot per box) so one day I fired up my furnace - melted it all down & poured it all into kilo bars & that 1,200 ozt sterling now fits in a medium flat rate box with room for 1/3 to half again more kilo bars (or room for another 350 - 500 ozt in the flat rate box)

The cost of shipping 1 or 2 or 3 or 4 regular large boxes - compared to shipping a small, medium or large flat rate box can make a big difference when it comes to silver

Bottom line - if/when I go to ship to a refinery I will save (make) money on just the shipping

Another way to put it - the kilo bars take up very little space in my gun safe - other wise I would have to store the larger boxes (of as is sterling) in the bottom of my closet &/or buy another safe just to store the silver

So (IMO) yes - if you are taking silver in small amounts to a pawn shop or coin dealer you are better off to NOT melt it --- on the other hand if you plan to send larger amounts (500 plus ozt) direct to a refinery you are better served pouring to bars

Kurt
 
Thank you both for your replies and constructive criticism.

Kurtak hit the nail on the head, this stuff takes a lot of space and it was already crowding my gun safe as it is. I live in Miami, Florida and i can tell you that any coin shop or pawnshop locally here will completely rip you off, buying or selling im talking 50 percent for sterling. I understand everyone has to make a profit but the premiums that they charge for buying and selling is so bad that its worth me to drive 2 hours for even a 200 dollar purchase or sale.

Having said that i will be selling directly to a refinery if and when i decide to sell and as kurtak mentioned they pretty much told me the same thing for sterling, they will do the melt and assay method anyway so it didnt matter how i brought it in. The same thing was going to happen for any silver that i refined myself so i thought it could hurt to get some practice in melting and pouring.

The goal would be to refine it myself with the method butcher posted, shot, nitric, cell. However im just not setup yet to do that safely and as you guys can imagine i wanted to get some part of this going or at least practiced.

Thank you again!
 
Another option for you is to trade your silver scrap for pure bullion!

https://goldrefiningforum.com/phpBB3/viewtopic.php?f=58&t=14782&hilit=scrapman#p156277

Take care! Phil
 
i saw scrapmans deal, and it is a good one. But i really want to learn this stuff plus its fun.

Going to put about another 100 troy through the furnace this week, well see how it goes.
 
Gsracer said:
i saw scrapmans deal, and it is a good one. But i really want to learn this stuff plus its fun.

Going to put about another 100 troy through the furnace this week, well see how it goes.


That's not a good deal anyway you slice it. Its almost scandalous we allow it on the forum your better off to go to the pawn shop. 47% is a crap premium with an assey charge of unmarked silver.

Eric

I have not had a bad deal with scrapman we did one 10 years ago.

I think if people were on here trying to buy gold like that they would be laughft out of here in a heartbeat.
 
philddreamer said:
Another option for you is to trade your silver scrap for pure bullion!

https://goldrefiningforum.com/phpBB3/viewtopic.php?f=58&t=14782&hilit=scrapman#p156277

Take care! Phil

I have never quite been able to figure out where scrapman's deal is a good deal --- in NO WAY am I saying it's a scam - he has offered terms for a trade & if you accept those terms - then it is a deal in terms of a "business" deal - I just don't see it as a good deal

To clarify - If a store is selling a product for $10 but I buy the same product from another store for $12 I didn't get scammed - I just didn't get the better deal --- such is the case here

The reason why I don't think scrapman's deal is a good deal (using the spot price of silver as of the time of this post)

Spot silver = $27.64 = 88 cent per gram (rounded down from actual .888)

If I sell direct to a refinery (based on a 500 ozt silver minimum) I get 95 % spot --- or 84 cents per gram or $26.12 ozt

Scrapman wants 47 grams silver in trade for a 1ozt (31.1) gram coin/round

47 grams silver (sold to refinery at 95% spot) is .84 X 47 = 39.48

I can go directly to Golden State Mint & buy 1 ozt coins/rounds from them for $30 each (price varies depending on type coin & quantity you buy)

Why would I pay (trade) $39.48 for the same coin I can buy direct from Golden State Mint at $30

Put another way ------

I can buy 500 ozt silver (coins/rounds) from GSM for $15,000

I would need to send a refinery 574.27 ozt silver to make $15,000 - which I could then buy the 500 ozt coins/round from GSM

I would need to send scrapman 755.6 ozt silver to get 500 ozt coins/rounds back


I could send that 755.6 silver to the refinery - get paid $19,834.50 - go buy 500 coins/rounds from GSM (for $15,000) - & end up with $4,834.50 in my pocket

Why would I make the trade :?:

Again - not saying scrapman is scamming anyone - he is making an open & honest business (trade) deal

I'm just not seeing where it is the best deal a person can make in the business of trading silver

Kurt
 
I think where scrapman deal comes into play is if you have relatively small quantities of scrap that well might fall under the amount needed to get a decent return from the refiners and those doing the trades are wanting stamped product rather than scrap or money.
From what I have seen on his thread most customers seem happy and the terms are clearly explained so the forum is happy to allow him to trade, as for advertising to buy or sell gold product it’s up to individuals to make an offer openly with what they are happy to accept or pay.
 
I agree, I have not traded any silver with scrap man, but I have heard nothing but praise from those who have, I have heard no complaints from his customers, it seems he has been honest in his dealings and that both parties are happy with the deals they have made.

It is not everyone that will acquire large volumes of silver scrap and learn enough to refine that silver to 999.9% by chemically using dangerous acids to recover the silver and then setting up and running an electrical cell, or they have better things to do like concentrating on collecting metals or learning to refine gold...

I feel scrap man has provided a service for those who wish to trade scrap for refined marked silver rounds, and do not wish to refine the scrap themselves and would prefer silver rounds much more easily traded or recognized for their value, and easier to stack in a hiding place.

I cannot speak for scrapman's rates, but I would suspect he is giving a better dealer return on the silver than the local pawn shops of bullion or scrap dealers, if not then I do not see where he would get any business from the members here.
 
He's also not hosing anyone on the assay either.

Go get 95% from your refiner on 30 ounces of your crap jewelry and tell me if it ain't really 88% after all the horecrap is done and over with.
 
Lou said:
He's also not hosing anyone on the assay either.

Go get 95% from your refiner on 30 ounces of your crap jewelry and tell me if it ain't really 88% after all the horecrap is done and over with.


Even if they shaft you with a 12% charge and not the 5% you know you should have. You will still come out better. Then you take you money and go to GSM and buy the same rounds for 10% premium with free shipping.

I'm not saying that he's scamming people. I am saying its a bad deal.




Eric
 
well in my defense, i was trying to be polite. As others have said it may be a great deal for some but it not for me. In either case, i get what you both are saying.
 
well back to my sterling bars, i got a scale that will measure up to 3000g by .1 gram. Its pretty accurate as all my standard weights where on the money up to 200 grams. So i threw in some of the mixed lots of sterling and a 10 oz bar and a 1.8 oz bar that came out poorly.

The pour and melt went pretty smooth with the procedure outlined above, I think this is the best bar ive poured to date.

Here are the pics

10.jpg
11.jpg
12.jpg
13.jpg
14.jpg
 
continuation

15.jpg

The before and after weight was 20.50 ozt troy, finished bar came in at 20.19 ozt when i got the left over out of the crucible it measure at .29 ozt leaving a melt loss of .04 ozt or 1.2grams. Im pretty happy with a 0.15% melt loss give or take

16.jpg

17.jpg


After i stamped the weight and cleaned it up. Got an interesting crystallization on cooling, i thought you would only see that on really high purity silver. Guess you can too on high purity sterling. lol


18.jpg

19.jpg
 
Doesn’t quite look the same as pure silver.
 

Attachments

  • DFAC4722-EC05-42AA-83F3-1F37D57D7E7A.jpeg
    DFAC4722-EC05-42AA-83F3-1F37D57D7E7A.jpeg
    4.3 MB · Views: 166
Lou said:
He's also not hosing anyone on the assay either.

Go get 95% from your refiner on 30 ounces of your crap jewelry and tell me if it ain't really 88% after all the horecrap is done and over with.

Lou - a couple things here

First off - yes - you are right - on a 30 ozt lot NO refiner is going to pay 95% - refineries generally have a sliding scale of payout based on lot size sent in (examples; - 85% if under 250 ozt - 90% if under 500 ozt - 95% 500 plus ozt) Those numbers can/do change (in percent &/or lot size) with different refiners

Also - most refiners have a minimum - under the minimum they will likely have assay frees (&/or other fees/charges) - over the minimum they generally wave those fees/charges

Second - there is no question about it - some refiners will flat out cheat you ("hidden" fees - "high" melt loss etc.) but there are certainly "honest" refiners out there --- over the years I have dealt with both (as in I have only dealt with two) the first one was cheating me - the second one (& the one I currently deal with) is honest

On the last lot of sterling I sent in (551 ozt of 925) I had 1.2 ozt melt loss (acceptable as far as I am concerned on 500 plus ozt) & I got their full 94% payout - NO fees/charges - so -----

I need to make bit of a correction here - yesterday (off the top of my head) I posted 95% - the refiner I am dealing with pays 94% on a minimum lot of 500 (plus) ozt of actual silver

Note for those still learning - when you send in a lot of sterling - the refiner pays on the amount of actual recovered 999 silver - so you need to send enough sterling (925) that the refiner will recover their minimum of refined 999 silver to get the full payment they offer

Bottom line - there is no question about it - there are some refiners out there that WILL screw you - but on the other hand there are certainly refiners out there that are honest - the trick is finding the honest ones

Examples; - the first refiner I dealt with was a cheater - the second one I found is & has been honest --- a very good friend of mine (he is a coin dealer & has been in business for many years) told me how he had to go through something like 3 - 4 refiners before he found an honest one - he has been happy & dealing with that refiner for years now

Kurt
 