pp2kr said:
Hello Sam
Tell us about your results!

pp2kr

The short version... it didn't really worked.
Perhaps some dissolution of gold, but not enough to make it a viable option..
 
Sam,, I am currently building a leach tank(4000 Ltr) , heated and insulated for au reduction in Glycine. it would be interesting to share notes on ur failures,,, success's in your trial. Btw ,, we dont have a Cu problem, will be using Hydrogen peroxide for di-oxy,, CuSO4 ( 4 nMol) 1 Mol Glycine. running thru a carbon collumn . cheers
 
There is a process for leeching using glycine, It looked a bit to me at a first glimpse as what they were aiming at.

A leeching process in the right PH range and at the right temp would work about that fast...

I will run this up in the lab tomorrow after my normally scheduled tomfoolery and see what happens. I think I have some glycine around...

Oh, and howdy guys, been reading for a while, never actually posted. I am rather impressed. I actually studied BioChem postgrad and well, ::coughs:: I hate to admit I am rather dodgy on actual knowledge of inorganic processing. I was more aimed at bio research, it has been lovely dusting off the cobwebs with you lads.

--L
 
Hi Fireflymetals and welcome to the forum.

Since your post mentioned glycine, I moved it to the glycine thread. :D

There are a couple of papers written about glycine leach, but it seems it isn't so specific to gold only.

Some articles that can be found via sci-hub.ac :
"The leaching of gold, silver and their alloys in alkaline glycine-peroxide solutions and their adsorption on carbon", E.A. Oraby, J.J. Eksteen, 2014, doi: 10.1016/j.hydromet.2014.12.015
"The selective leaching of copper from a gold–copper concentrate in glycine solutions", E.A. Oraby, J.J. Eksteen, 2014, doi: 10.1016/j.hydromet.2014.09.005

Looks like they are experimenting with it in Australia.

Let us know how it goes, so far I haven't heard anyone else trying glycime on the forum.

Göran
 
So, while I have tonnes of odd things in my kit, I did not have glycine...

I ordered it and it showed up today, was packing things up to wander into the lab and got a call informing me that there was no power in the building, so results will be delayed.

I played a bit with modeling software (it never answers anything but it gives you good basal parameters).

Long story short, the answer is delayed...

I was planning on answering in the other thread (thanks for moving this), I also found datum I will post over there.

In any case I will keep you all appraised of what comes from this, I expect to have the experiment up and running in about 48 hours.

For datum points however I will run down what the process is going to be:

I have 4 items up on this weeks bench.

For testing I have 40kg of tight trimmed gold fingers. (I hear people having problems sourcing volumes of items. I don't know why I found that part easy but there ya go).


Glycine leaching: Testing 500 grams, looks like I will be working in a 5l beaker and starting with roughly 1l of leechant (I over shoot needs due to the fact that I prefer big batches).
Recovery will be carbon and I will be doing a ash out, water plunge separation then tossing the remains in the small furnace for a melt out. I should get a lil bead out of that.

More as it comes along.

--L
 
I do not know if my input will help but you need to keep the solution heated, I think the temperature is fairly critical, and moving constantly to effectively strip the gold the same as using weak cyanide solutions, also from the little I understand of this method it will not load as much gold as cyanide so running a winning cell would allow the solution to be stripped of values and pumped back into the leach tank providing the movement, I'm not sure how the cell will react to the glycine so more may have to be added if it destroys some or all of it.
As I stated earlier this method has legs but the details at present are sketchy and I think testing is going to be needed to make the process work effectively, it also looks like this process will need specific equipment such as pumps to provide flow, a cell to strip the solution and almost certainly access to assaying to determine the effectiveness of the stripping and recovery, short version is this will not be for a hobbyist or home refiner until the process is proved.
 
I have a very specific and unusual Gold coated Silica ore . I use the Simple Glycine hydrogen peroxide leach at +/- 150 deg F. . I still have to figure out how
to post photos. My pregnant leach has a reddish color to it giving me the impression of Colloidal Gold . I pass a red Laser beam thru the loaded leach and
get a clear line thru the leach , no defusion of the light . My Activated Carbon
increases by 16 grams per 1pound in my carbon column when I have dried the loaded AC . I am unable to elute the Gold from the Activated Carbon (AC )
I am able to recover the Gold by destroying the Glycine leach, turning it into
Chloride . I welcome new ideas
 
You can practice in the Private message area.

Click on "Private message" up toward the upper right corner of the window.

Then click on "Compose message" from the menu list along the left side.

You can type a little text, attach a couple of images, and hit the "Preview" button to see how it looks. Play with the "Place inline" button.

The PM editing screen is pretty close to the Post editing screen. If you click on the "Submit" button by mistake, it will just give you an error that you didn't specify a subject or a recipient (don't ask me how I know :oops: ). I built a couple of my large projects that way.

Dave
 
Hi all,
Wanted to chime in here as I've been doing a lot of reading both on the forums and academic literature over the past few months and finally decided to register and contribute.
My background is a decade as an electrical engineer with a lifetime passion for chemistry, so I'm doing my best to use my career knowledge of the initial production process of what becomes ewaste to optimize my feedstock processing and selection.

I am still doing my "getting started" required reading and am abstaining from using strong acids until I know I have all safety measures in place. That being said, I decided to give alkaline glycine leaching a try since I'm comfortable with NaOH form prior soapmaking experience.

My feedstock is some trimmed PCI card and RAM stick fingers, as well as some trimmed down mylar flex PCBs from old cell phones that have what is likely ENIG gold on some of the ground planes.

I've been trying different ratios of H2O2 and glycine molarity (no more than 1M solution) along with constant stirring at room temperature, and I'm finding decent, albeit slow, success dissolving the base metals out from under the gold foils. I'm taking my time and waiting until I have more gold foils before I try a refining of the gold via higher temperature alkaline glycine process as outlined in literature.

I had an idea to use copper to drop out the other base metals in the waste glycine solutions and indeed immediately saw what I believe is nickel cement out on some pieces of copper plate placed in the copper glycinate filtrate. I'm hoping to figure out something to be able to drop out the copper in a way that preserves the glycine for reuse, though the only mention in literature I've found is sodium hydrosulfide, which I would prefer not to work with at this time. Perhaps there is a way to acidify the solution, use sodium metabisulfite to drop the copper, and then increase the pH again, without degradation of the solution.

Anyway, I've attached some photos, apologies for the quality, I took them simply for personal documentation at the time and wasn't expecting to post them.
That being said, I'm grateful for this place and how willing everyone is to share knowledge.

- Mare
 

Attachments

  • 2024-12-21 10_35_33.png
    2024-12-21 10_35_33.png
    16.6 MB
  • 2024-12-21 10_35_52.png
    2024-12-21 10_35_52.png
    13.7 MB
Hi all,
Wanted to chime in here as I've been doing a lot of reading both on the forums and academic literature over the past few months and finally decided to register and contribute.
My background is a decade as an electrical engineer with a lifetime passion for chemistry, so I'm doing my best to use my career knowledge of the initial production process of what becomes ewaste to optimize my feedstock processing and selection.

I am still doing my "getting started" required reading and am abstaining from using strong acids until I know I have all safety measures in place. That being said, I decided to give alkaline glycine leaching a try since I'm comfortable with NaOH form prior soapmaking experience.

My feedstock is some trimmed PCI card and RAM stick fingers, as well as some trimmed down mylar flex PCBs from old cell phones that have what is likely ENIG gold on some of the ground planes.

I've been trying different ratios of H2O2 and glycine molarity (no more than 1M solution) along with constant stirring at room temperature, and I'm finding decent, albeit slow, success dissolving the base metals out from under the gold foils. I'm taking my time and waiting until I have more gold foils before I try a refining of the gold via higher temperature alkaline glycine process as outlined in literature.

I had an idea to use copper to drop out the other base metals in the waste glycine solutions and indeed immediately saw what I believe is nickel cement out on some pieces of copper plate placed in the copper glycinate filtrate. I'm hoping to figure out something to be able to drop out the copper in a way that preserves the glycine for reuse, though the only mention in literature I've found is sodium hydrosulfide, which I would prefer not to work with at this time. Perhaps there is a way to acidify the solution, use sodium metabisulfite to drop the copper, and then increase the pH again, without degradation of the solution.

Anyway, I've attached some photos, apologies for the quality, I took them simply for personal documentation at the time and wasn't expecting to post them.
That being said, I'm grateful for this place and how willing everyone is to share knowledge.

- Mare
Welcome
 
Hi all,
Wanted to chime in here as I've been doing a lot of reading both on the forums and academic literature over the past few months and finally decided to register and contribute.
My background is a decade as an electrical engineer with a lifetime passion for chemistry, so I'm doing my best to use my career knowledge of the initial production process of what becomes ewaste to optimize my feedstock processing and selection.

I am still doing my "getting started" required reading and am abstaining from using strong acids until I know I have all safety measures in place. That being said, I decided to give alkaline glycine leaching a try since I'm comfortable with NaOH form prior soapmaking experience.

My feedstock is some trimmed PCI card and RAM stick fingers, as well as some trimmed down mylar flex PCBs from old cell phones that have what is likely ENIG gold on some of the ground planes.

I've been trying different ratios of H2O2 and glycine molarity (no more than 1M solution) along with constant stirring at room temperature, and I'm finding decent, albeit slow, success dissolving the base metals out from under the gold foils. I'm taking my time and waiting until I have more gold foils before I try a refining of the gold via higher temperature alkaline glycine process as outlined in literature.

I had an idea to use copper to drop out the other base metals in the waste glycine solutions and indeed immediately saw what I believe is nickel cement out on some pieces of copper plate placed in the copper glycinate filtrate. I'm hoping to figure out something to be able to drop out the copper in a way that preserves the glycine for reuse, though the only mention in literature I've found is sodium hydrosulfide, which I would prefer not to work with at this time. Perhaps there is a way to acidify the solution, use sodium metabisulfite to drop the copper, and then increase the pH again, without degradation of the solution.

Anyway, I've attached some photos, apologies for the quality, I took them simply for personal documentation at the time and wasn't expecting to post them.
That being said, I'm grateful for this place and how willing everyone is to share knowledge.

- Mare
Copper will only drop the precious metals and Mercury if present.
 
An update on my experiments, I have figured that the dissolution of nickel in an alkaline glycine leach is fairly pH dependent, and it can be left as a solid by keeping the pH below ~9 or so. Above that it goes into solution via complexing just as copper does. This explains the black coloration on some of the gold foils I have been recovering.

As for the cementing out in my waste liquids, I think it was just a trick of the eye of viewing copper metal through a deep blue solution.

While I wait for various processes I have been continuing to educate myself and the info on this forum has helped the copper chloride process finally click for me, and I can certainly see the benefits it has for a hobbyist refiner due to the ways it regenerates and can be refreshed.

That being said, I am setting up some copper electrowinning cells to see if it is possible to to recover the dissolved copper, as well as regenerate the glycine ligands in solution. I know other ways of recovering copper in literature have been shown to leave the glycine unaffected, but those methods involve using sodium hydrosulfide, which I would prefer not to use at this time. If the electrowinning works, it would be fairly straightforward to setup a two tank, closed loop system. One tank for the stripping of copper to liberate the foils, and the other tank to electrowin the copper and regenerate the lixiviant. I think if the pH were maintinated well enough, the selectivity for copper could keep the nickel used in the ENIG and hard gold processes attached to the foils, and that nickel could be leached and recovered separately in another set of tanks, though the yields would be quite a bit lower I would imagine.
 
So I setup a little test cell just to make sure that the copper glycinate solution is a suitable electrolyte, and I was able to demonstrate proof of concept that indeed I can plate copper onto a stainless cathode. I used a copper anode to test while I wait for my titanium sheets to arrive. I'm hoping that the titanium will successfully plate out the copper while remaining unreactive in the alkaline glycinate solution. If all that goes well, it's just a matter of testing the depleted solution in the cell for it's ability to dissolve more copper off on input material, which will confirm the preservation of the glycine zwitterion in solution, and approach a closed loop system aside from electricity in the electrowinning cell, and air bubbling through the leach solution.

The paper I referenced is this one here. Unfortunately it's not open, so I can't share the PDF, but in summary:
Leach solution is 1M glycine 1M sodium carbonate, input material is PCBs ground and seived, solid/liquid concentration is 5g solid/200mL solution, mechanical stirring during leaching process. For the electrodeposition they use a stainless steel anode and cathode, as well as a reference electrode for their metrology methods.

Compared to my procedure I used KOH to increase the pH, so if I run into issues with the electrodeposition I will likely try leaching again using a solution the same as the one in the paper.
 

Attachments

  • IMG_6052.jpg
    IMG_6052.jpg
    3.7 MB
  • IMG_6051.jpg
    IMG_6051.jpg
    2.8 MB
Last edited:
For anyone interested in why this isn't feasible as a closed loop process paired with electrowinning for recovering copper (and freeing gold) from PCBs (information from a mix of experimental data and review of literature):
  • Stainless steel anodes likely contaminate the solution with Cr3+ ions (and possible other alloying metals like Molybdenum)
  • Lead anodes cannot be used as they can complex with glycine leading to lead glycinate in solution and degradation of the anodes
  • Platinized titanium anodes catalyticly oxidize glycine at the anode to form formaldehyde as well as other hazardous compounds, and render the solution non-recyclable
    • I found no mention of it but I have no reason not to think that more expensive iridium oxide/tantalum interlayer/titanium anodes would behave any differently
  • Using an intermediate solvent extraction to move the copper to a sulfate-based electrolyte (allowing for more traditional copper electrowinning processes) is not only more complicated, the extraction solvents are highly toxic, not readily available (only have seen this used/mentioned: LIX-84), and also degrade the glycine content of the leach solution
There are few-to-no advantages to using alkaline glycine leach to recover copper and free gold from ewaste over the copper chloride ('AP') process as far as I can tell. This even applies to feed stock as minorly-heterogenous as trimmed gold fingers.

As for the glycine method for actual gold recovery and processing, with literature describing a 1mg/L saturated solution in ideal circumstances with optimized parameters, running a 1000L/g of gold system seems fairly unapproachable for the home player.

It's possible that this new-ish process will be improved upon to a point where it makes sense on a small scale, but as of now, it's a novelty for the hobbyist at best.

Basically: more of what everyone else has been saying.

At least my curiosity is sated. Time to cement out all my waste, process it accordingly, and move on to other things.

EDIT: going over my notes I'm realizing I never tried a carbon electrode. Not optimistic about its possibilities but I suppose using it with an anode bag to catch the deteriorating carbon particles could be viable. That is, assuming it doesn't cause degradation of the glycine.
 