More specifically Sodium Hypochlorite.Chlorox is Hypochlorite
Anything else you want to inform us about?
More specifically Sodium Hypochlorite.Chlorox is Hypochlorite
and followed that up by saying this,I precipitate PGM's and base metals out of Aqua Regia with an Alloy of Aluminum and Magnesium, then I selectively leach different base metals out
The 2 processes you have mentioned will produce different, if not questionable results. I am afraid that anyone trying to follow this thread will be thrown off without clarification.In my experience, I find Palladium chloride and Silver chloride co-precipitate when you add Salt to the Aqua Regia
While I do not understand the mechanism for just table salt dropping the Palladium I will concur that Silver Chloride is notorious for dragging down other metals with it and possibly, in your case, Palladium is dragged down.Now filter the Silver Chloride out of the Aqua Regia Solution, and wash this with clean water until the water becomes clear. Now Filter the water away. Leach the water-free Silver Chloride with Hydrochloric acid/ Chlorox , you will find that the leach will turn orange, meaning that Palladium is extracted from the Silver Chloride.
maybe you mean that they co-precipitate when you add salt to the solution of Pd and Ag in nitric acid (not in AR). I seem to remember that it also happened to me on one occasion.in my experience, I find Paladium chloride and Silver chloride co-precipitate when you add Salt to the Aqua Regia
Is better to chase the platinum from two solutions than the gold. If you inquart the gold too much below 25% then it too will follow the silver into solution. Inquarting with copper is gods way of punishing the cheap for being lazy. I tell my people all the time that procedure is written in order for a reason. Until and unless you understand why it is in the order as written it is best to not adjust unless you want to have a mess on your hands. This green solution is a mess and it is going to fight you for the value it contains. I know I will catch hell for this but if you are inquarting with copper then you are wrong. If you have to do it so be it, but its more expensive and will waste more material in the end. If your pgms will follow silver into solution, then why would they not follow copper?The classic assay books tell you in order to get all of the PGM's away from the Gold you should inquart with Silver at 10 times the Platinum content to allow it all to follow the Silver. That also implies making the Gold 25% or less. But the texts do specify this will cause all of the Platinum to migrate over. But if your parting has less than 10 times the Silver as Platinum there will be Platinum on both sides of the equation, meaning some Platinum remaining with the Gold and some Platinum following the silver. From a practical refining method, chasing PGM's two different ways is not efficient.
The inquartation with Silver to allow all of the Platinum to follow the Silver is only a reasonable option if @100tific has a Silver cell operating to recover the Platinum after cementing the Silver and any PGM's with copper and running it in a cell.
The aqua regia option would be my choice after lowering the Silver content below 9-10% with copper. The gold should be dropped first and with that much copper added it will not come down clean. It will need a second aqua regia refine.
Wether or not the copper causes issues with dropping PGM's completely if the copper completely dissolved it should not as cementation works on metallic copper. If it were me, I would cement the PGM's on copper, and a clean copper slab would work for this as well. Then, once the original solution is barren of values, the insolubles should be filtered and digested in aqua regia and the Platinum recovered either by ammonium chloride or cementing with sparing additions of copper powder.
As far as the Jahn-Teller effect is concerned it is commonly seen in transition metal complexes so copper does apply. The exact effect the Jahn-Teller effect will have on this particular reaction is subject for debate, there are so many variables that present themselves in acid refining that determining that would be a difficult process. Seeing as you have an alloy and apparently a customer or boss that wants to see the refined metal to sell it, I think the Jahn-Teller effect is a wormhole that may absorb your efforts for a very long time. On the bright side, your research may re-define refining as we know it and your efforts may result in a Nobel prize. Considering Nobel prizes in chemistry are awarded overwhelmingly to men, I would be happy to see it!
Sodium chloride in AR should not participate silver chloride under any circumstances. It would be created from the chloride in the hcl alone.In what form does the Pd precipitate?
Absolutely true.Sodium chloride in AR should not participate silver chloride under any circumstances. It would be created from the chloride in the hcl alone.
Palladium co-precipitation was also my first bet.I should point out that you really should not be drying the ammonium hexachloroplatinate like that. It is best to always handle it damp, with full PPE and preferably in a filter box. Then take a shower after!
That admonition aside, the color of the ammonium hexachloroplatinate you have shown and talked about indicates contamination. It's highly suggested to either dissolve the salt in aqua regia (or otherwise remove the ammonium cation) and complete a hydrolytic refining from oxidizing conditions, as described in 4metals other thread titled Bromate Hydrolysis. You do not need to use bromate, chlorine and caustic soda are use industrially. Bromate just happens to give a better result.
the iridate salt, which comes down substantially completely with the platinum from highly oxidized solutions, will darken your platinum precipitate orange to red. Palladium can also do this, and is far more likely.
With amounts of platinum and palladium in material, I would suggest (as other experienced members suggested) to go for the gold and accumulate PGM residue for later processing. Working with PGMs is much more complex and tedious task, and it is best to combine the leftovers from multiple runs to save time and your sanitymaybe you mean that they co-precipitate when you add salt to the solution of Pd and Ag in nitric acid (not in AR). I seem to remember that it also happened to me on one occasion.
thank you very much kurt and 4metals.
There were some things I didn't know like not using AR if PGMs are not the main metal, or that PGMs don't precipitate well in dilute solutions. Also the silver 10 times higher than the Pt so that it drags everything towards the silver part.
You are not aware of what a tremendous pleasure it is to read and learn from you.
I will reconsider everything you have told me and see again what path to take.
I come across platinum tunings more often than I would like and sometimes I don't understand why sometimes it turns out well and other times not so much.
So thanks again for providing your vision.
I take this opportunity to ask another question. I have noticed that sometimes the precipitate after adding ammonium chloride is yellow, other times orange, and even once I recovered it from a solution that had iridium it came out red. From what I have read, this depends on the temperature at which it is formed. But as I understand it, iridium precipitates black. The red I got was carmine red, it didn't look like a mixture of the orange powder and black. I leave a photo of the normal one, and that red that I tell you about. In case you can provide some valuable information through your experience.
Thanks guys
![]()
![]()
![]()
all images are ammonium hexachloroplatinate
Nitric will not touch Pt, unless it is alloyed with Silver.hello I just put my two cents here, I read you and I learned a lot, personally I never went through aqua regia if AG Above 7%, too many jokes in the past, too much loss and too much processing time afterwards (to be avoided and prohibited).Nitric acid dissolves platinum in small concentrations ????
oh good??
why then do I find the exact grammage even when it's 3gr per kg?? especially in silver blocks that I etch with nitric 65%?
Unless I'm not washing properly, which is possible because I was never allowed to breathe in boulor, I find that with NH4Cl I usually get pure platinum at 996.5/1000. never 999.9 (DAMN!)
for my part and fans of your case, I would have :
1) passage HNO3 -----> Ag and Pd degage
2) filtration -----> Ag/Pd filtrate / retained solid: Au/Pt
3) The filtrate would then be treated in several ways depending on your equipment:
a) precipitation on Cu -----> melting ----> shot blasting-> Ag cell
Ag recovery in 999.9 and Pd recovery in “sludge”.
I'd do a silver cell electrolyte test especially if green tint, if pd present then Dmg and recovery.
to finish, sponge and pd sludge in AR----> precipitation on Cu or zinc powder works very well.
b) Add HCL OR NaCl ---->Ag recover in agcl form ----> Naoh---->glucose----> Ag 999.9 IF rinse well and compress after each wash, to avoid precipitate of Agcl you have to mix several times, its structure changes and it becomes finer, you have to let it rest and filter it, it is important to be meticulous.
View attachment 66543
View attachment 66545
image way b)
View attachment 66544
Pd solution remains ------> Cu precipitation, OR DMG or wholtech method.
4) Coming back to the Au/Pt solid not attacked by HNO3, I'd like to point out that platinum is never attacked in my laboratory, perhaps because I always add enough H2O to cover the alloy to be attacked before adding the nitric acid, perhaps because the nitric acid dissolved in this way doesn't attack it (something to think about).
Take your solids, wash well with distilled H2O several times.
Once well washed, I check for any trace of Agcl still present by adding a little Hcl to the distilled water I used to wash the remaining solids. If Agcl is still present, wash again with hot water.
5) passage of solids in AR, another small detail,
I never prepare aqua regia 1/4 HNO3--3/4 HCL (c'est bon pour les durs à cuire) ici on recherche la finesse, l'élégance et la clarté. Bref, soyez un vrai gentleman cambrioleur.
SO put enough HCL 37% (muratic acid) that you think you need, and THEN add little by little HNO3 repeatedly, until complete dissolution.
SO put enough HCL 37% (muratic acid) that you think you need, and THEN add HNO3 little by little repeatedly, until the solids are completely dissolved. Why I do this, to simply avoid having to denox HNO3. I therefore approach the stoichiometric quantities
6) After that, nothing could be simpler when you find yourself dear friends with your liquor containing dissolved Au and Pt, you can therefore proceed in 2 different steps:
a) ajouter du sulfate de fer (II = vert) pour précipiter l'Au----> filtration----> lavage avec HCL 37%-- deuxième filtration -----> lavage à l'eau distillée ----> séchage ---> fonte. L'Au est sorti OUI !!!!!
View attachment 66542
There will therefore only be the platinum left and you can precipitate it with ammonium chloride, before precipitating it you can also add hydrochloric acid, which you used to rinse your gold, in fact it sometimes happens that a little platins follow Au, it is therefore found in hcl that you used to wash it.
To turn your platinum sponge into metal you can either heat it delicately, slowly to avoid losing any, then once it is very black, melt it, or redissolve it and this time precipitate it with formic acid.
View attachment 66539
here is the appearance of my sponge, 996.5/1000
as I do not like to lie and I love to share my discoveries it is often accompanied by results in order to prove the veracity of my results and what is so lacking in your forum, people put forward hypotheses without controlling their results .
small contamination Pd Rh because waiting to much time before filtration
View attachment 66541
View attachment 66540
my face : always work with security , becareful about Pt et Pd sponge.
I would like to make an interesting remark, there is no one on the forum who has taken the time to explain how to correctly refine platinoids and I find that really shameful, I would like the main speakers to take the time to do so a thread on this subject whether in the patent or library section, I am sure that some have the knowledge, the knowledge and the adequate tools to do it so wait you stop keeping your secrets in a cupboard, we must move forward together, and even if your boss forbids you to do it, break the silence, it is not us who are going to compete with an LBMA or any foundry lost on the other side of the world, so advice to the specialists hiding and not sharing, help us progress
see you
Welcome to us.Hi there,
Thanks for sharing your process! The green scab you observed is likely CuCl₂ (Copper(II) chloride), formed due to the high copper content reacting with chloride ions in aqua regia. This can happen if the reaction slows or becomes less acidic over time.
To confirm, dissolve a small amount in water—CuCl₂ is water-soluble and turns the solution green.
Since copper is dominating, it might interfere with dissolving other metals. You could filter the residue and consider removing excess copper (e.g., via cementation with iron) before continuing with platinum and gold recovery.
Let me know if you need further tips!
On the other hand Copper will not "interfere" with dissolving other metals.Hi there,
Thanks for sharing your process! The green scab you observed is likely CuCl₂ (Copper(II) chloride), formed due to the high copper content reacting with chloride ions in aqua regia. This can happen if the reaction slows or becomes less acidic over time.
To confirm, dissolve a small amount in water—CuCl₂ is water-soluble and turns the solution green.
Since copper is dominating, it might interfere with dissolving other metals. You could filter the residue and consider removing excess copper (e.g., via cementation with iron) before continuing with platinum and gold recovery.
Let me know if you need further tips!
I am fascinated by your explanation, thank you very much. I think your Pt never follows nitric because the amount of silver is not 10 times greater than that of platinum.hello I just put my two cents here, I read you and I learned a lot, personally I never went through aqua regia if AG Above 7%, too many jokes in the past, too much loss and too much processing time afterwards (to be avoided and prohibited).Nitric acid dissolves platinum in small concentrations ????
oh good??
why then do I find the exact grammage even when it's 3gr per kg?? especially in silver blocks that I etch with nitric 65%?
Unless I'm not washing properly, which is possible because I was never allowed to breathe in boulor, I find that with NH4Cl I usually get pure platinum at 996.5/1000. never 999.9 (DAMN!)
for my part and fans of your case, I would have :
1) passage HNO3 -----> Ag and Pd degage
2) filtration -----> Ag/Pd filtrate / retained solid: Au/Pt
3) The filtrate would then be treated in several ways depending on your equipment:
a) precipitation on Cu -----> melting ----> shot blasting-> Ag cell
Ag recovery in 999.9 and Pd recovery in “sludge”.
I'd do a silver cell electrolyte test especially if green tint, if pd present then Dmg and recovery.
to finish, sponge and pd sludge in AR----> precipitation on Cu or zinc powder works very well.
b) Add HCL OR NaCl ---->Ag recover in agcl form ----> Naoh---->glucose----> Ag 999.9 IF rinse well and compress after each wash, to avoid precipitate of Agcl you have to mix several times, its structure changes and it becomes finer, you have to let it rest and filter it, it is important to be meticulous.
View attachment 66543
View attachment 66545
image way b)
View attachment 66544
Pd solution remains ------> Cu precipitation, OR DMG or wholtech method.
4) Coming back to the Au/Pt solid not attacked by HNO3, I'd like to point out that platinum is never attacked in my laboratory, perhaps because I always add enough H2O to cover the alloy to be attacked before adding the nitric acid, perhaps because the nitric acid dissolved in this way doesn't attack it (something to think about).
Take your solids, wash well with distilled H2O several times.
Once well washed, I check for any trace of Agcl still present by adding a little Hcl to the distilled water I used to wash the remaining solids. If Agcl is still present, wash again with hot water.
5) passage of solids in AR, another small detail,
I never prepare aqua regia 1/4 HNO3--3/4 HCL (c'est bon pour les durs à cuire) ici on recherche la finesse, l'élégance et la clarté. Bref, soyez un vrai gentleman cambrioleur.
SO put enough HCL 37% (muratic acid) that you think you need, and THEN add little by little HNO3 repeatedly, until complete dissolution.
SO put enough HCL 37% (muratic acid) that you think you need, and THEN add HNO3 little by little repeatedly, until the solids are completely dissolved. Why I do this, to simply avoid having to denox HNO3. I therefore approach the stoichiometric quantities
6) After that, nothing could be simpler when you find yourself dear friends with your liquor containing dissolved Au and Pt, you can therefore proceed in 2 different steps:
a) ajouter du sulfate de fer (II = vert) pour précipiter l'Au----> filtration----> lavage avec HCL 37%-- deuxième filtration -----> lavage à l'eau distillée ----> séchage ---> fonte. L'Au est sorti OUI !!!!!
View attachment 66542
There will therefore only be the platinum left and you can precipitate it with ammonium chloride, before precipitating it you can also add hydrochloric acid, which you used to rinse your gold, in fact it sometimes happens that a little platins follow Au, it is therefore found in hcl that you used to wash it.
To turn your platinum sponge into metal you can either heat it delicately, slowly to avoid losing any, then once it is very black, melt it, or redissolve it and this time precipitate it with formic acid.
View attachment 66539
here is the appearance of my sponge, 996.5/1000
as I do not like to lie and I love to share my discoveries it is often accompanied by results in order to prove the veracity of my results and what is so lacking in your forum, people put forward hypotheses without controlling their results .
small contamination Pd Rh because waiting to much time before filtration
View attachment 66541
View attachment 66540
my face : always work with security , becareful about Pt et Pd sponge.
I would like to make an interesting remark, there is no one on the forum who has taken the time to explain how to correctly refine platinoids and I find that really shameful, I would like the main speakers to take the time to do so a thread on this subject whether in the patent or library section, I am sure that some have the knowledge, the knowledge and the adequate tools to do it so wait you stop keeping your secrets in a cupboard, we must move forward together, and even if your boss forbids you to do it, break the silence, it is not us who are going to compete with an LBMA or any foundry lost on the other side of the world, so advice to the specialists hiding and not sharing, help us progress
see you
What is the point of waiting for smb gases if you are going to precipitate it with copper anyway?The most economical way to handle this if you absolutely had to work with the copper diluted alloy would be to completely dissolve it in AR and then drop the gold. If smb was used to drop the gold you would need to let the solution rest in the open atmosphere for a few days to make sure the sulfur containing gases were gone from the solution.
Then cement the values so you can get a clean solution to work with when you add Ar again.