Silver oxide, caustic soda and sugar

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

Ellorath

Member
Joined
Jul 31, 2015
Messages
8
Hi guys,

Can anyone help me with the complete reactions of AgCl to solid Ag. I just couldn't find it anywhere.. :roll:

Thanks!!
 
Hi again,

I have seen in the videos, that first caustic and then adding syrup to the mixture. I want to understand it in reaction steps. I would appreciate so much if you guys write the reactions in steps like what happens first adding caustic and then syrup.

Thanks:)
 
Ellorath said:
Hi again,

I have seen in the videos, that first caustic and then adding syrup to the mixture. I want to understand it in reaction steps. I would appreciate so much if you guys write the reactions in steps like what happens first adding caustic and then syrup.

Thanks:)

The bit you missed off was "thanks guys for the answer to the question I asked." 8) 8)
 
I can understand the inorganic chemistry fairly well, but here we are dealing with organic chemistry, which is a different ball game, Someone with an understanding of organic chemistry can better explain just how the glucose is converted to gluconate during the reduction of silver salt to metal.
I do believe Lou has discussed this in his earlier posts on the subject.
 
2 AgCl + 2 NaOH -> 2NaCl + Ag2O + H2O


Ag2O + C6H12O6 + NaOH → 2 Ag + C6H11O7Na + H2O


Global
2 AgCl + C6H12O6 + 3 NaOH -> 2 Ag + C6H11O7Na + 2 H2O + 2 NaCl

Glucose to sodium gluconate
 
If it is interesting someone, some silver oxide is complexed in the soluble state, NaAg(OH)2
 

Attachments

  • Silver (1) solubility.jpg
    Silver (1) solubility.jpg
    72.9 KB
Lino1406 said:
If it is interesting someone, some silver oxide is complexed in the soluble state, NaAg(OH)2

I would like to hear more on this subject!
 
Silver is one of the Amphoteric metals, which can dissolve in excess basic solutions.
So I can see where some of the silver would be soluble if excess caustic is used to oxidize the silver.

https://en.wikipedia.org/wiki/Amphoterism
http://dwb5.unl.edu/chem/smallscale/SmallScale-078.html
 
Sometimes, but not always i get a hint of silver chloride when washing silver with hcl after a silver chloride/NaOH/sugar conversion.
 
Hi again,

Sorry I am new here and will learn the code:)
Thank you all for sharing great information with me! May the gold be with you! Amen :D :G