Stirring in the presence of iron didn’t work for me. I still had agcl present.
I had to tumble the silver chloride with iron as the grinding media.
You need intimate contact between the agcl and the iron.
Sent from my iPhone using Tapatalk
I had to tumble the silver chloride with iron as the grinding media.
You need intimate contact between the agcl and the iron.
Sent from my iPhone using Tapatalk