Hi everyone i need some advice to improve this work for large-scale and speed up the process

Here is my work

1. Someone asked me to recover gold from slag sample .

2. The slag came from gold-laden carbon that was smelted with copper and charcoal.

3. I used aqua regia to dissolve the sample after I crushed it.

4. The result was a gelatinous liquid with floating tiny white particles.

5. It was very hard to filter it, but I did it patiently.

6. I used sodium metabisulfite to precipitate gold from the resulting liquid.

7. The gold was suspended in the solution like nanoparticles.

8. I let it settle, but some gold was still present in the solution.

9. I tried a pretreatment with nitric acid, and again the gelatinous precipitate appeared.

10. This time, I saw little shiny gold at the bottom of the beaker.

11. I discarded the gelatinous solution by decantation and dissolved the gold in aqua regia.

The total sample was 600g.

The first run was 400g and yielded 1g of gold.

The second run was a 200g sample, yielding 0.5g of gold.

My problem was the gelatinous solution, which may have trapped some gold inside it. How can I get rid of it?

And how can I make the small gold particles coagulate together?

When I started to read CM Hoke, she mentioned that this book does not cover this issue.

Sorry for my English and for being overly verbose.
 

Attachments

  • IMG_20241009_170043.jpg
    IMG_20241009_170043.jpg
    3.2 MB
  • IMG_20241010_171051.jpg
    IMG_20241010_171051.jpg
    2.4 MB
  • IMG_20241010_173300.jpg
    IMG_20241010_173300.jpg
    2.5 MB
  • IMG_20241010_210111.jpg
    IMG_20241010_210111.jpg
    2.3 MB
  • IMG_20241010_210154.jpg
    IMG_20241010_210154.jpg
    2.3 MB
  • IMG_20241010_183122.jpg
    IMG_20241010_183122.jpg
    2.2 MB
Hi everyone i need some advice to improve this work for large-scale and speed up the process

Here is my work

1. Someone asked me to recover gold from slag sample .

2. The slag came from gold-laden carbon that was smelted with copper and charcoal.

3. I used aqua regia to dissolve the sample after I crushed it.
Maybe it should have been incinerated first, it seems to be very high in Carbon still.


4. The result was a gelatinous liquid with floating tiny white particles.
Do you know which Flux they used? Maybe you should have boiled it in weak Sulfuric first to remove as much Flux as possible.


5. It was very hard to filter it, but I did it patiently.

6. I used sodium metabisulfite to precipitate gold from the resulting liquid.
Did you get any proper Gold precipitation? Did you test with Stannous?


7. The gold was suspended in the solution like nanoparticles.
That may be a sign of too low concentration or too much base metals.

8. I let it settle, but some gold was still present in the solution.

9. I tried a pretreatment with nitric acid, and again the gelatinous precipitate appeared.

10. This time, I saw little shiny gold at the bottom of the beaker.

11. I discarded the gelatinous solution by decantation and dissolved the gold in aqua regia.
How do you treat your waste?


The total sample was 600g.

The first run was 400g and yielded 1g of gold.

The second run was a 200g sample, yielding 0.5g of gold.

My problem was the gelatinous solution, which may have trapped some gold inside it. How can I get rid of it?

And how can I make the small gold particles coagulate together?

When I started to read CM Hoke, she mentioned that this book does not cover this issue.

Sorry for my English and for being overly verbose.
Do you know how it was treated before it came to you?

Comments in bold inside the Quote.

I think much can be fixed by proper pre-treatment.
I'd start with crushing the slag as you do but very fine, then boil it with weak Sulfuric 10-20% ish, check what flux they used during smelting.
Then I'd dry it well and incinerate it to get rid of the Carbon.
Then it should be ready for AR.
Make/get some Stannous so you can test your solution.
During precipitation if it won't settle, add a bit of Sulfuric and boil it hard for a while.
This seems to promote forming bigger particles and more complete settling.

This should be a starting point at least.
 
Do you know how it was treated before it came to you?

Comments in bold inside the Quote.

I think much can be fixed by proper pre-treatment.
I'd start with crushing the slag as you do but very fine, then boil it with weak Sulfuric 10-20% ish, check what flux they used during smelting.
Then I'd dry it well and incinerate it to get rid of the Carbon.
Then it should be ready for AR.
Make/get some Stannous so you can test your solution.
During precipitation if it won't settle, add a bit of Sulfuric and boil it hard for a while.
This seems to promote forming bigger particles and more complete settling.

This should be a starting point at least.
The flux they used was "sodium bicarbonate and sodium tetraborate decahydrate"

I will try this tonight,
I have stannous chloride test and it give me positive with AR




 
The flux they used was "sodium bicarbonate and sodium tetraborate decahydrate"

I will try this tonight,
I have stannous chloride test and it give me positive with AR
If there is still carbon left it will grab some of your Gold.
The Carbon should be properly ashed before smelting.
 
But how to ash large amounts of slag maybe 10kg for one run in large scale it would be very hard
You need to check if the black color is from Carbon or something else.
Talk with the ones creating the slag.

If they are smelting without ashing they most likely have heavy losses.
Dissolving the surplus salts from the slag by boiling in dilute Sulfuric or even plain water should be your first step.
 