Hello
I have been trying this for past few months and found it to be useful and easy to recover Ag from Ag NO3 using Cu powder
I tried for few days and now i want to share with all of you
I could recover 15-25Kg of Ag in just 15-20mins
This is my precipitating vessel
This is my precipitating vessel with stirrer
on left side of vessal there is stirrer which has black handle with PP sheet at its bottom
After putting AgNO3 in vessel and add Cu powder. and stir the sol you will see Ag in tank
you can check Ag is fully recovered by adding Hcl to it if white spots apper after adding Hcl means Ag is Still In Sol
so add Bit more Cu These you hav to do till all Ag is precipitated
I may not be clear in above process
I will try to add video soon.
If any queries ple feel free to ask
Hrushi
I have been trying this for past few months and found it to be useful and easy to recover Ag from Ag NO3 using Cu powder
I tried for few days and now i want to share with all of you
I could recover 15-25Kg of Ag in just 15-20mins
This is my precipitating vessel
This is my precipitating vessel with stirrer
on left side of vessal there is stirrer which has black handle with PP sheet at its bottom
After putting AgNO3 in vessel and add Cu powder. and stir the sol you will see Ag in tank
you can check Ag is fully recovered by adding Hcl to it if white spots apper after adding Hcl means Ag is Still In Sol
so add Bit more Cu These you hav to do till all Ag is precipitated
I may not be clear in above process
I will try to add video soon.
If any queries ple feel free to ask
Hrushi