Looking for learning,

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.
I new in this indduusstry, just learning, seeing video on Youtube, and faild 2 times, :)
I'm here hope to find what I miss, please support
Welcome to us.
Point 1 Youtube is not a good teacher.
Point 2 We need more information, what have you tried to do.
Point 3 you need to study more obviously.

Give us some more information and we can start helping you.

In the mean time study these links:

We ask our new members to do 3 things.
1. Read C.M. Hokes book on refining jewelers scrap, it gives an easy introduction to the most important chemistry regarding refining.
It is free here on the forum: https://goldrefiningforum.com/phpBB3/viewtopic.php?f=54&t=19798
2. Then read the safety section of the forum: https://goldrefiningforum.com/forums/safety.47/
3. And then read about "Dealing with waste" in the forum: https://goldrefiningforum.com/threads/dealing-with-waste.10539/

Suggested reading:
https://goldrefiningforum.com/forums/the-library.101/
https://goldrefiningforum.com/threads/when-in-doubt-cement-it-out.30236/
https://goldrefiningforum.com/threa...le-read-this-before-you-post-about-ore.33333/


Forum rules is here.
https://goldrefiningforum.com/threads/gold-refining-forum-rules.31182/
 
Hi,
I'm happy to share my issue:
I have plates with 3 layer: gold, Niken and Copper and I start refining gold step by step as below:
Step 1: Immerse in a solution of nitric acid and water to separate the gold layers. After seeing that the gold layer has completely separated from the plate, I filter it through absorbent paper and obtain the gold-plated layer.
Step 2: I put the filter paper with the gold layer into the aqua regia solution (3HCL + HNO3) with heat, I tried to add as little HNO3 as possible by dropping until the metal was completely dissolved. After the metal was completely dissolved, I filtered the dissolved solution.
Step 3: I add in the same amount of water as the solution and boil until the water level returns to normal then let it cool, my purpose is to remove the HNO3
Step 4: I add SMB the solution, it turn to dark colour
After time, the solution appears precipitate but it stays cloudy and muddy, very soluble, i have attached a picture for you, i tested the water with stannous chloride and it turned black
Should I filter out this precipitate, boil the solution and continue adding SMB until I see a yellow precipitate or is there any other solution? Please advise.
 

Attachments

  • acf53b14566aef34b67b8.jpg
    acf53b14566aef34b67b8.jpg
    243 KB
  • b988e97a84043d5a641512.jpg
    b988e97a84043d5a641512.jpg
    608.3 KB
  • d993510b3c75852bdc647.jpg
    d993510b3c75852bdc647.jpg
    470.8 KB
  • 28539caef1d0488e11c19.jpg
    28539caef1d0488e11c19.jpg
    549 KB
  • 652030d25dace4f2bdbd11.jpg
    652030d25dace4f2bdbd11.jpg
    611.4 KB
  • da15f1e29c9c25c27c8d10.jpg
    da15f1e29c9c25c27c8d10.jpg
    675 KB
Hi,
I'm happy to share my issue:
I have plates with 3 layer: gold, Niken and Copper and I start refining gold step by step as below:
Step 1: Immerse in a solution of nitric acid and water to separate the gold layers. After seeing that the gold layer has completely separated from the plate, I filter it through absorbent paper and obtain the gold-plated layer.
Step 2: I put the filter paper with the gold layer into the aqua regia solution (3HCL + HNO3) with heat, I tried to add as little HNO3 as possible by dropping until the metal was completely dissolved. After the metal was completely dissolved, I filtered the dissolved solution.
Step 3: I add in the same amount of water as the solution and boil until the water level returns to normal then let it cool, my purpose is to remove the HNO3
Step 4: I add SMB the solution, it turn to dark colour
After time, the solution appears precipitate but it stays cloudy and muddy, very soluble, i have attached a picture for you, i tested the water with stannous chloride and it turned black
Should I filter out this precipitate, boil the solution and continue adding SMB until I see a yellow precipitate or is there any other solution? Please advise.
Well you can start reading the links I gave you.
In Step 3 this do not work at all.
If you are going to do it by evaporation.
You need to evaporate to a thick syrupy consistence.
Then add HCl.
Brown funes should evolve if there still is Nitric in there.
If so do it again.
Whan the Nitric and NOx is driven off.
Add HCl until all is dissolved and filter until crystal clear.

Then add SMB and the Gold should drop just fine. Then test with Stannous.
If it test negative you can set it aside until next day. Test it again then if it is still negative, decant the liquid and collect the powder on the bottom.
If needed refine again.
 
Well you can start reading the links I gave you.
In Step 3 this do not work at all.
If you are going to do it by evaporation.
You need to evaporate to a thick syrupy consistence.
Then add HCl.
Brown funes should evolve if there still is Nitric in there.
If so do it again.
Whan the Nitric and NOx is driven off.
Add HCl until all is dissolved and filter until crystal clear.

Then add SMB and the Gold should drop just fine. Then test with Stannous.
If it test negative you can set it aside until next day. Test it again then if it is still negative, decant the liquid and collect the powder on the bottom.
If needed refine again.
Sure I will read all the link,
But in this case, could you advise me now I should filter the brown precipitate,then start HCL process OR leave them there and start HCL process?
thank you for your respone
 
Sure I will read all the link,
But in this case, could you advise me now I should filter the brown precipitate,then start HCL process OR leave them there and start HCL process?
thank you for your respone
Have you tested with Stannous?
Have you tested the pH?
 
Have you tested with Stannous?
Have you tested the pH?
Hi,
I filtered the solution to 2 part:
Part 1 is the brown precipitate: I put to AR and Test Stannous give very black colour
Part 2 is the remain solution in liquid: I test Stannous also give black colour but less than Part 1
So I start solve 2 part as:
Part 1: I add HCL and water and boild to kill HNO3 , then add SMB but precipitate still not hard, i attach picture, please advise me
Part 2: U add HCL and boil to a thick syrupy consistence.
please give me your opinions
 

Attachments

  • 040b2a2097242e7a773518.jpg
    040b2a2097242e7a773518.jpg
    716.8 KB
  • b2a64b72f6764f28166717.jpg
    b2a64b72f6764f28166717.jpg
    400.1 KB
Hi,
I filtered the solution to 2 part:
Part 1 is the brown precipitate: I put to AR and Test Stannous give very black colour
Part 2 is the remain solution in liquid: I test Stannous also give black colour but less than Part 1
So I start solve 2 part as:
Part 1: I add HCL and water and boild to kill HNO3 , then add SMB but precipitate still not hard, i attach picture, please advise me
Part 2: U add HCL and boil to a thick syrupy consistence.
please give me your opinions
Stannous will give purple to black if there are Gold, it is our eyes in refining to know if there is still Precious metals in solution.
You need to decompose Nitric NOx before SMB and boiling will not do that.
You need to evaporate to syrup and then add HCl.
After doing this one or more times it is ready to drop it after it is filtered clean.
This should give a clean and complete drop of Gold.
This is how a stannous test look like:
Picture from Lazersteve
1728367768280.png
 
Stannous will give purple to black if there are Gold, it is our eyes in refining to know if there is still Precious metals in solution.
You need to decompose Nitric NOx before SMB and boiling will not do that.
You need to evaporate to syrup and then add HCl.
After doing this one or more times it is ready to drop it after it is filtered clean.
This should give a clean and complete drop of Gold.
This is how a stannous test look like:
Picture from Lazersteve
View attachment 65231
Ygg. A Nitric solution decomposes with heat.
 
Do it decompose enough by just boiling that it can be used effectively?
If so why did Ms. Hoke go to such lenghts?
In fairness Deano used to tell me that you keep it hot till no brown fumes come off as a main starting point and then the precipitant can deal with any residual Nitric. It does work too. Remember Hoke was written specifically for people who weren't delving into the whys and wherefores, and to provide a sure and repeatable path.

This doesn't contradict Hoke, it's merely additional useful info.
 
In fairness Deano used to tell me that you keep it hot till no brown fumes come off as a main starting point and then the precipitant can deal with any residual Nitric. It does work too. Remember Hoke was written specifically for people who weren't delving into the whys and wherefores, and to provide a sure and repeatable path.

This doesn't contradict Hoke, it's merely additional useful info.
Yes, but now I was guiding one of the guys you describe.
 
It all comes down to the question of how much nitric was left over after the reaction. One mistake many refiners make is adding too much nitric acid and failing to eliminate it before dropping the gold. I believe that is the case here.

When I did a large aqua regia digestion in a heated reactor, I always let the heat continue until the reaction stopped blowing off the red NOx and then, as Deano suggested to Jon, the reaction of the precipitant will consume any small amount of remaining nitric. It does this by dropping the gold and the remaining nitric re-dissolves what you just dropped and consumes any free nitric. This continues until the nitric is gone and the precipitation can go on to completion. This is not unlike the trick Jon's old friend Harold used to use which was adding a chunk of refined gold to react with and consume any remaining nitric.

This is not effective (the heating) if there was simply much too much nitric to begin with. Considering how hard and costly it is to get nitric acid, it surprises me how many members (mostly new to refining) over use it.
 
See Ygg? *sticks tongue out and waggles it* :love:

In seriousness though as 4metals clarified- if people use way too much, then it doesn't lend itself to getting rid of the Nitric this way. The cyclic precipitate/dissolve reaction with precipitants can be used to effectively take out the last Nitric, just as the button does.
 
See Ygg? *sticks tongue out and waggles it* :love:

In seriousness though as 4metals clarified- if people use way too much, then it doesn't lend itself to getting rid of the Nitric this way. The cyclic precipitate/dissolve reaction with precipitants can be used to effectively take out the last Nitric, just as the button does.
I think bubbling SO2 through it will take care of any Nitric residues while in the end dropping the Gold.
 
The best, by far, application of SO2 gas I have ever worked with is using a system called surface effect gassing. I know this is way beyond the means of most refineries but the video seen HERE gives exceptional detail and a good overall idea of how their system works.

As I said, not for most but still enlightening to see in practice.
 