bluestar
New member
- Joined
- May 9, 2016
- Messages
- 3
I attached some fun pictures.
Solution:
11.3 grams of 99%+ when into 50ml HCL and leached with 5 ml hno3 slowly added.
I have leached using 1.6 volts and no HNO3, but it's not worth it.
No additives
Anode was 99%+ gold
Ti cathode marked with a 50w CO2 laser. No really impressed with the result, but it was really easy.
Cathode cleaned with Bar Keepers Friend
Voltage floated from 0.25-0.3 at a constant 0.2 amps
Plates out at about 2.5-3 grams per amp hour.
Solution:
11.3 grams of 99%+ when into 50ml HCL and leached with 5 ml hno3 slowly added.
I have leached using 1.6 volts and no HNO3, but it's not worth it.
No additives
Anode was 99%+ gold
Ti cathode marked with a 50w CO2 laser. No really impressed with the result, but it was really easy.
Cathode cleaned with Bar Keepers Friend
Voltage floated from 0.25-0.3 at a constant 0.2 amps
Plates out at about 2.5-3 grams per amp hour.