VolkD
Active member
I've done this before. By dissolving 300g of sodium persulfate in 1L of hydrochloric acid. In 52 hours I didn't notice any gold tarnishing. If I left it long enough, it would probably show, but in practice I do everything in about 6 hours.Since you're doing all this as an experiment, may I suggest you take some of the bits of gold foils you recover and put them in some fresh HCl and add some fresh persulfate. Let us know how that turns out after soaking it for a couple of days.
Edit, add:
Otherwise, there is already an AP method that dissolves some gold if you use peroxide. Sodium persulfate probably also eats some gold. Otherwise, very very little, but I'm happy to pay for speed.
Last edited: