So I melt my silver in a graphite crucible in a resistive heating furnace.

If my cement silver is pure I do not observe any sputtering and the melt is well behaved.

But if my cement silver is impure(close to 80%) I observe a lot of spluttering and I see a lot of silver attached to the lid of the furnace the sputtering subdues after some time.

I'm pretty sure I'm not the first one observing the phenomena id like to know what other members use to avoid such sputtering(if something like this is possible) and why is it the sputtering only occurs for impure silver while the pure silver(98-99%) behave very well(no sputtering).
 
So I melt my silver in a graphite crucible in a resistive heating furnace.

If my cement silver is pure I do not observe any sputtering and the melt is well behaved.

But if my cement silver is impure(close to 80%) I observe a lot of spluttering and I see a lot of silver attached to the lid of the furnace the sputtering subdues after some time.

I'm pretty sure I'm not the first one observing the phenomena id like to know what other members use to avoid such sputtering(if something like this is possible) and why is it the sputtering only occurs for impure silver while the pure silver(98-99%) behave very well(no sputtering).
I don't know of any other methods other than to re-dissolve the silver and make it purer.
:)
I have seen that silver cement is also pressed into tubes (for example, using a syringe) and they are melted, so it is less likely to scatter....
 
I don't know of any other methods other than to re-dissolve the silver and make it purer.
:)
I have seen that silver cement is also pressed into tubes (for example, using a syringe) and they are melted, so it is less likely to scatter....

The sputtering I mention off is during the molten state.
 
This is usually because of reactions with impurities during the melt.
If there are Oxides, Nitrates or other substances present, there can be many "interesting" reactions.

This is my best guess, aided by the fact I am using a graphite crucible.
Would adding borax to the melt reduce the sputtering...?
 
This is my best guess, aided by the fact I am using a graphite crucible.
Would adding borax to the melt reduce the sputtering...?
If it creates a "lid" on the melt it can contain it maybe.
But I'm not sure how well Borax plays with Graphite.

What kind of impurities do you have in there?
 
If it creates a "lid" on the melt it can contain it maybe.
But I'm not sure how well Borax plays with Graphite.

What kind of impurities do you have in there?

If it creates a "lid" on the melt it can contain it maybe.
But I'm not sure how well Borax plays with Graphite.

What kind of impurities do you have in there?

Majority of it being copper.
 
There is no reason that clean Copper should cause this.
Are there Oxides, Nitrates or moisture in it?
Moisture WILL cause explosions like this.

I do admit I have moisture in my melt, but I'm not sure why is it only there in the impure melt, my clean cement silver 98-99% does not exhibit such explosions.
 
There is no reason that clean Copper should cause this.
Are there Oxides, Nitrates or moisture in it?
Moisture WILL cause explosions like this.

Yes oxides for sure I am very confident I have oxides in my melt something that could not be washed by hot water rinse, the reason for impure silver
 
This is my best guess, aided by the fact I am using a graphite crucible.
Would adding borax to the melt reduce the sputtering...?
Borax loves to consume Graphite crucibles. Pure Graphite crucibles should only be used for metals. A silica/Alumina crucible is better suited for your melts. All components of the melt should be dry, to reduce the amount of steam expulsion.
 
Borax loves to consume Graphite crucibles. Pure Graphite crucibles should only be used for metals. A silica/Alumina crucible is better suited for your melts. All components of the melt should be dry, to reduce the amount of steam expulsion.
Also try adding a bit of Carbon to the melt. Flour works wonders on Oxides. About 1 gram per 11 grams of oxides ( not already reduced metals ).
 
Also try adding a bit of Carbon to the melt. Flour works wonders on Oxides. About 1 gram per 11 grams of oxides ( not already reduced metals ).

This is what I get as the first search result.
They sure are not on the cheaper side.
 

Attachments

  • Screenshot_20250206-095600_Google.jpg
    Screenshot_20250206-095600_Google.jpg
    499.4 KB
Those are the best available. I don't know what the exchange rate is to US dollars. There are a lot of manufacturers here in the states, where A/S crucibles are fairly cheap. DFC ceramics in Colorado is very reasonable, Legend in Nevada is an OK source also. Buying in bulk is always cheaper. I buy them in case lots (50 - 1 assay ton ) for I think around 3-4.00 each. I think you could probably melt Tungsten in the screen shot crucibles.
 
not sure how you are heating the crucible. if you can start on low heat and ramp up the heat steadily and slow you might be able to drive the moisture off and then allow you to get a full melt. I suspect there is trapped moisture in your material or trapped air. Good luck.

Maybe ball mill your material first then heat it slowly.
 
Thanks for all the replies.
I do agree the moisture is my melt is an issue and is always a good practice to remove the same, but what interests me the my cement silver that is pure does not exhibit such sputtering even when moist.
 
Yes, molten silver readily absorbs oxygen from the air, a phenomenon known as "spitting of silver" where the absorbed oxygen is released violently as the silver solidifies, causing small silver particles to be ejected; this is why precautions are often taken when working with molten silver to prevent this issue.

Key points about molten silver and oxygen absorption:
  • Significant absorption:
    Molten silver can absorb a large volume of oxygen, sometimes up to 20 times its own volume.

  • Cooling release:
    When the molten silver cools and solidifies, the absorbed oxygen is released rapidly, causing the "spitting" effect.

  • Prevention methods:
    To mitigate spitting, I use a sealed furnace for my melts to help prevent oxygen absorption. I've read you can use a thin layer of charcoal on the molten silver, but I've never tried it.
 

Latest posts