Wash off the silver coating in concentrated sulfuric acid.

Gold Refining Forum

Help Support Gold Refining Forum:

This site may earn a commission from merchant affiliate links, including eBay, Amazon, and others.

anarxi

Well-known member
Joined
Oct 30, 2019
Messages
318
used:
2 glasses with a capacity of 1 liter.
700 milliliters sulfuric acid 92%
80 milliliters nitric acid 58%
Tap water for rinsing: about 15 liters.

base material
copper, brass, bronze with silver plating.
 

Attachments

  • IMG_20241027_210624445_MP.jpg
    IMG_20241027_210624445_MP.jpg
    2.1 MB
  • IMG_20241027_210242601_BURST002.jpg
    IMG_20241027_210242601_BURST002.jpg
    1.3 MB
  • IMG_20241027_144353491_MP.jpg
    IMG_20241027_144353491_MP.jpg
    1.8 MB
  • IMG_20241027_143404139_MP.jpg
    IMG_20241027_143404139_MP.jpg
    1.1 MB
  • IMG_20241027_171237447_MP.jpg
    IMG_20241027_171237447_MP.jpg
    139 KB
  • IMG_20241027_143357292_MP.jpg
    IMG_20241027_143357292_MP.jpg
    2.1 MB
  • IMG_20241028_201026815_MP.jpg
    IMG_20241028_201026815_MP.jpg
    939.5 KB
OK you have created a pretty strong solution that effectively and selectively will strip Silver plating. Now how are you recovering the Silver from the solution? Half of a solution to a problem is as bad as no solution.
 
OK you have created a pretty strong solution that effectively and selectively will strip Silver plating. Now how are you recovering the Silver from the solution? Half of a solution to a problem is as bad as no solution.
Well, I didn't create it.
This is an old classic solution from the beginning of the last century.
at least.
in the classics, for 19 parts of sulfuric acid there is 1 part of nitric acid.
transformation of silver through chloride.
the solution (a mixture of acids + dissolved metals, silver and tin, zinc, possibly bismuth) is simply poured into salt water.
I pour it into a canister containing water from previous work.
through the neck into which the watering can is inserted.
sulfuric acid and water, as you know, behave violently when combined.
you need a gas mask (or goggles and a respirator) and rubber, durable gloves.
 