kadriver
Well-known member
I started on this today using Harold's PDF as a guide
I found diamonds and other stones and pulled them prior to incinerating.
I did not do this screening because I don't have any screens yet.
I did the magnetic treatment by putting a magnet into a thick plastic bag, there was very little magnetic material to remove.
I incinerated using the pyroceramic Corning ware dish because I could not find a stainless steel pan at the thrift store as of yet.
The incineration went well and everything was heated to redness with a low flame from propane torch while the casserole was on high heat.
I did a stannous test on the nitric and there's some gold and Pt in solution - I goofed early on and added HCl instead of nitric!
Had to dry everything out and re-incinerate, but there was probably some residual HCl that caused some gold and Pt to go into solution.
There is a little Pt filings in this batch.
Back to the shop, I'll put some photos up later.
The next step is to inquart and I am at a loss here on how much silver to add - educated guess. Any input would be greatly appreciated.
kadriver
I found diamonds and other stones and pulled them prior to incinerating.
I did not do this screening because I don't have any screens yet.
I did the magnetic treatment by putting a magnet into a thick plastic bag, there was very little magnetic material to remove.
I incinerated using the pyroceramic Corning ware dish because I could not find a stainless steel pan at the thrift store as of yet.
The incineration went well and everything was heated to redness with a low flame from propane torch while the casserole was on high heat.
I did a stannous test on the nitric and there's some gold and Pt in solution - I goofed early on and added HCl instead of nitric!
Had to dry everything out and re-incinerate, but there was probably some residual HCl that caused some gold and Pt to go into solution.
There is a little Pt filings in this batch.
Back to the shop, I'll put some photos up later.
The next step is to inquart and I am at a loss here on how much silver to add - educated guess. Any input would be greatly appreciated.
kadriver