Hi to All,
Ok where to begin! I guess with the specs of my cell,so here they are.
POWER SUPPLY(Front Panel)
Radio Shack
Regulated 12 volt Power supply
Converts 120 VAC to 12 VDC
1 on/off power switch
POWER SUPPLY(Back Panel)
120 VAC
60 HZ
60 WATTS MAX
OUTPUT 13.8 VDC- 2.5A
3 AMP reset switch
2 wires & 2 clamps
1 gallon pickle jar
ANODE and CATHODE (any SILVERPLATE WARE you choose)
ELECTROLYTE(good old H2O)
Ok now to the process .
1.Fill jar about 3-5 inches from the top so you have plenty of room for rinseing periodically .
2.Clamp Anode and Cathode to jar (Leave Anode+ half out of water helps deplate better).Do not let your clamps touch the water.
3.Make sure that Anode and Cathode are across from one another ,not side by side.
4.Turn power supply on,after about 1 1/2 minutes you should start seeing the silver coming off in a cloudy stream.
5.After it runs for a hour or two the cell will start to get real cloudy and by this time you,ll start to see growth on the anode (don,t panic) just power the cell off .
6.Use spray bottle and tooth brush to clean Anode (Make sure to do this back into the cell).Do not clean Cathode.
7.Flip Anode around so deplated end is sticking out of water and reclamp, and turn power back on.
8.When second half is done , turn power off ,unclamp Anode and use it to stir the cell for about a minute then clean second half of Anode then replace with new Anode.Continue steps 2-8 Until step 9 comes into play.
9.When water is almost to the top near clamp, power down remove and clean current Anode,remove and spray only the Cathode(You want Cathode to stay tarnished black).
10.Now that cell is pregnant filter all liquid through 3 stacked coffee filters 1 time only.
11.Rinse black powder in filter with spray bottle, dry till it hardens then save for bigger melt.
12.Now refill cell with the same fluid you filtered and start again,except now you can leave Anode in for longer time period and let the growth grow longer before cleanings.
Heres my video
https://www.youtube.com/watch?v=1WCyoq1yMgg