Yes definitely expect small crystals as ams said. After a few days they should beef up. The power supply your using is basically the same as mine, it should work with no issues.
Looks like your getting it sorted out. That’s great.
To help visualize the connections and anodes this is what i use..
Try to go 10 gauge. I have found even at low amps 14 gauge heads up and start to drop voltage at the cell.
You can pour a small bar with a piece of silver hammered into a wire. I make my anodes out of cement silver.
That way if they drop into the cell, no worries. Its just refining the silver i already wanted to refine.
Looks like your getting it sorted out. That’s great.
To help visualize the connections and anodes this is what i use..
Try to go 10 gauge. I have found even at low amps 14 gauge heads up and start to drop voltage at the cell.
You can pour a small bar with a piece of silver hammered into a wire. I make my anodes out of cement silver.
That way if they drop into the cell, no worries. Its just refining the silver i already wanted to refine.